e01.org

Animal Proteins

578,848 chars · English

The Project Gutenberg eBook of Animal Proteins

This eBook is for the use of anyone anywhere in the United States and
most other parts of the world at no cost and with almost no restrictions
whatsoever. You may copy it, give it away or re-use it under the terms
of the Project Gutenberg License included with this eBook or online
at www.gutenberg.org. If you are not located in the United States,
you will have to check the laws of the country where you are located
before using this eBook.

Title: Animal Proteins

Author: Hugh Garner Bennett

Release date: October 26, 2012 [eBook #41192]
Most recently updated: October 23, 2024

Language: English

Other information and formats: www.gutenberg.org/ebooks/41192

Credits: Produced by Juliet Sutherland, Joanna Johnston and the
Online Distributed Proofreading Team at http://www.pgdp.net
(This file was produced from images generously made
available by The Internet Archive/Million Book Project)

*** START OF THE PROJECT GUTENBERG EBOOK ANIMAL PROTEINS ***

Transcriber's Note:

Minor typographical errors and inconsistencies have been corrected. Some
words had inconsistent hyphenation throughout the book; these have been
made consistent.

In the mathematical and chemical expressions, the caret character
represents "to the power of", e.g. e^2 means e-squared. Curly braces are
used to represent underscores, e.g. n{1} means n with a subscript of 1.
Equal signs are used to represent =bold words=, and underscores are used
to represent italics.

On page 152 NaCO{23} has been corrected to Na{2}CO{3}. On page 212,
the variable n has been replaced with the correctly subscripted forms
n{1} and n{2}.

The index entry for Hemlock bark had no page number in the original
text, so the correct page number, 34, has been supplied.

Ions are shown as Fe+++, instead of using superscripts.

There is some inconsistency in the notation used in the original text
for chemical formulae such as Na{2}Cr{2}O{7}(2H{2}O). These have
been regularized to use the modern mid-dot, for example,
Na{2}Cr{2}O{7}·2H{2}O.

Greek letters in the original have been represented in this version by
the name of the letter enclosed in square brackets, e.g. [alpha].

ANIMAL PROTEINS

BY

HUGH GARNER BENNETT, M.Sc. (LEEDS)

MEMBER OF THE SOCIETY OF LEATHER TRADES' CHEMISTS; FORMERLY ASSISTANT
LECTURER AND DEMONSTRATOR AT THE LEATHER INDUSTRIES DEPARTMENT OF THE
UNIVERSITY OF LEEDS

AUTHOR OF "THE MANUFACTURE OF LEATHER"

LONDON

BAILLIÈRE, TINDALL AND COX 8, HENRIETTA STREET, COVENT GARDEN
1921

(_All rights reserved_)

GENERAL PREFACE

The rapid development of Applied Chemistry in recent years has brought
about a revolution in all branches of technology. This growth has been
accelerated during the war, and the British Empire has now an
opportunity of increasing its industrial output by the application of
this knowledge to the raw materials available in the different parts of
the world. The subject in this series of handbooks will be treated from
the chemical rather than the engineering standpoint. The industrial
aspect will also be more prominent than that of the laboratory. Each
volume will be complete in itself, and will give a general survey of the
industry, showing how chemical principles have been applied and have
affected manufacture. The influence of new inventions on the development
of the industry will be shown, as also the effect of industrial
requirements in stimulating invention. Historical notes will be a
feature in dealing with the different branches of the subject, but they
will be kept within moderate limits. Present tendencies and possible
future developments will have attention, and some space will be devoted
to a comparison of industrial methods and progress in the chief
producing countries. There will be a general bibliography, and also a
select bibliography to follow each section. Statistical information will
only be introduced in so far as it serves to illustrate the line of
argument.

Each book will be divided into sections instead of chapters, and the
sections will deal with separate branches of the subject in the manner
of a special article or monograph. An attempt will, in fact, be made to
get away from the orthodox textbook manner, not only to make the
treatment original, but also to appeal to the very large class of
readers already possessing good textbooks, of which there are quite
sufficient. The books should also be found useful by men of affairs
having no special technical knowledge, but who may require from time
to time to refer to technical matters in a book of moderate compass,
with references to the large standard works for fuller details on
special points if required.

To the advanced student the books should be especially valuable. His
mind is often crammed with the hard facts and details of his subject
which crowd out the power of realizing the industry as a whole. These
books are intended to remedy such a state of affairs. While
recapitulating the essential basic facts, they will aim at presenting
the reality of the living industry. It has long been a drawback of our
technical education that the college graduate, on commencing his
industrial career, is positively handicapped by his academic knowledge
because of his lack of information on current industrial conditions. A
book giving a comprehensive survey of the industry can be of very
material assistance to the student as an adjunct to his ordinary
textbooks, and this is one of the chief objects of the present series.
Those actually engaged in the industry who have specialized in rather
narrow limits will probably find these books more readable than the
larger textbooks when they wish to refresh their memories in regard to
branches of the subject with which they are not immediately concerned.

The volume will also serve as a guide to the standard literature of the
subject, and prove of value to the consultant, so that, having obtained
a comprehensive view of the whole industry, he can go at once to the
proper authorities for more elaborate information on special points, and
thus save a couple of days spent in hunting through the libraries of
scientific societies.

As far as this country is concerned, it is believed that the general
scheme of this series of handbooks is unique, and it is confidently
hoped that it will supply mental munitions for the coming industrial
war. I have been fortunate in securing writers for the different
volumes who are specially connected with the several departments of
Industrial Chemistry, and trust that the whole series will contribute
to the further development of applied chemistry throughout the Empire.

SAMUEL RIDEAL.

AUTHOR'S PREFACE

It has been the author's chief concern that this volume should fulfil
its own part in the programme set forth in Dr. Rideal's General Preface.

The leather, glue, and kindred trades have been for many years
recognized as chemical industries, but the great development of colloid
chemistry in the last few years has given these trades a more definite
status as such, and they can now be placed in the category of applied
physical chemistry. The time is probably not far distant when some
knowledge of pure physical chemistry will be a first essential to
students, chemists, chemical engineers, and to all engaged in these
industries in supervision, administration, or control. It is hoped that
this volume will stimulate the study of these industries from that
standpoint.

As the author has previously written upon one of the industries involved
herein ("The Manufacture of Leather": Constable & Co.), he has, rather
inevitably, found it difficult to avoid altogether his own phraseology.
The changes of a decade, however, together with the wider field and
newer view-point, have made possible a radical difference of treatment.

The author desires to acknowledge the help he has received from the many
books, essays, and researches which are mentioned in the references at
the end of each section, especially to Procter's "Principles of Leather
Manufacture," and also to thank Dr. Rideal for many useful suggestions.
The author would like also to acknowledge here his indebtedness (as well
as that of the trade generally) to the work of Dr. J. Gordon Parker, who,
through his researches, lectures, and teaching work, has done more than
any other man to disseminate a knowledge of practical methods of
tanning.

The author's thanks are also due to his brother, Mr. W. Gordon Bennett,
M.Sc., A.I.C., M.C., for assistance in proof revision, and to his
father, Rev. John Bennett, for some literary criticism.

H. GARNER BENNETT.
BEVERLY, _June_, 1921.

CONTENTS

GENERAL PREFACE

AUTHOR'S PREFACE

CONTENTS

INTRODUCTION

* * * * *

PART I.

HIDES FOR HEAVY LEATHERS.

SECTION

1. THE RAW MATERIAL OF HEAVY LEATHERS

2. THE PREPARATION OF PELT

3. VEGETABLE TANNAGE

4. FINISHING PROCESS

5. SOLE LEATHER

6. BELTING LEATHER

7. HARNESS LEATHER

8. UPPER LEATHERS

9. BAG LEATHER

10. PICKING BAND BUTTS

* * * * *

PART II.

SKINS FOR LIGHT LEATHERS.

1. PRINCIPLES AND GENERAL METHODS OF
LIGHT LEATHER MANUFACTURE

2. GOATSKINS

3. SEALSKINS

4. SHEEPSKINS

5. CALFSKINS

6. JAPANNED AND ENAMELLED LEATHERS

* * * * *

PART III.

CHROME LEATHERS.

1. THE NATURE OF CHROME LEATHERS

2. GENERAL METHODS OF CHROME LEATHER
MANUFACTURE

3. CHROME CALF

4. CHROME GOAT AND SHEEP

5. HEAVY CHROME LEATHERS

* * * * *

PART IV.

MISCELLANEOUS TANNAGES.

1. ALUM TANNAGES

2. FAT TANNAGES

3. OIL TANNAGES

4. FORMALDEHYDE TANNAGE

5. SYNTHETIC TANNING MATERIALS

6. COMBINATION TANNAGES

7. THE EVOLUTION OF THE LEATHER INDUSTRY

* * * * *

PART V.

GELATINE AND GLUE.

1. PROPERTIES OF GELATINE AND GLUE

2. RAW MATERIALS AND PRELIMINARY
TREATMENT

3. EXTRACTION

4. CLARIFICATION AND DECOLORIZATION

5. BLEACHING

6. EVAPORATION

7. COOLING AND DRYING

8. USES OF GELATINE AND GLUE

9. THE EVOLUTION OF THE GELATINE AND
GLUE INDUSTRY

* * * * *

PART VI.

MISCELLANEOUS PROTEINS AND BYE-PRODUCTS.

1. BYE-PRODUCTS OF THE LEATHER TRADES

2. BYE-PRODUCTS OF THE GELATINE AND
GLUE TRADES

3. FOOD PROTEINS

4. MISCELLANEOUS ANIMAL PROTEINS

INDEX

ANIMAL PROTEINS

INTRODUCTION

Proteins are organic compounds of natural origin, being found in plants
and in animals, though much more plentifully in the latter. They are
compounds of great complexity of composition, and of very high molecular
weight. The constitution of none of them is fully understood, but
although there are a great number of different individual proteids, they
present typical resemblances and divergences which serve to
differentiate them from other groups of organic bodies, and also from
one another.

Proteins resemble one another in both proximate and ultimate analysis.
They contain the usual elements in organic compounds, but in proportions
which do not vary over very wide limits. This range of variation is
given approximately below:--

Element. Per cent.

Carbon 49 to 55
Hydrogen 6.4 to 7.3
Oxygen 17 to 26
Nitrogen 13 to 19
Sulphur 0.3 to 3.0

The most characteristic feature of the protein group is the amount of
nitrogen usually present. This is generally nearer the higher limit,
seldom falling below 15 per cent. This range for the nitrogen content is
determined largely by the nature of constituent groups which go to form
the proteid molecule. Roughly speaking, proteins consist of chains of
amido-acids and acid amides with smaller proportions of aromatic groups,
carbohydrate groups and thio compounds attached. In these chains an acid
radical may combine with the amido group of another amido acid, the acid
group of the latter combining with an amido group of another amido acid,
and so on. Hydrogen may be substituted in these chains by alkyl or
aromatic groups. There is obviously infinite possibility of variation in
constitution for compounds of this character, the general nature of
which varies very little. Practically all of the proteins are found in
the colloid state, and this makes them very difficult to purify and
renders the ultimate analysis in many cases doubtful. It is, for
example, often difficult to ascertain their moisture content, for many
are easily hydrolyzed with water only, and many part easily with the
elements of water, whilst on the other hand many are lyophile colloids
and practically cannot be dehydrated or dried. A few, such as gelatin
and some albumins, have been crystallized.

The constituent groups have been investigated chiefly by hydrolytic
methods. The chains of amido acids are split up during hydrolysis, and
individual amido acids may thus be separated. The hydrolysis may be
assisted either by acids, alkalies or ferments, but follows a different
course according to the nature of the assistant. Under approximately
constant conditions of hydrolysis, the products obtained are in
approximately constant proportions, and this fact has been utilized by
Van Slyke in devising a method of proximate analysis. It is not possible
in this volume to enter deeply into the constitution of the different
proteids. Reference must be made to works on pure chemistry, especially
to those on advanced organic chemistry. It will be interesting, however,
to mention some of the amido acids and groups commonly occurring in
proteids. These comprise ornithine (1:4 diamido valeric acid), lysine
(1:5 diamido-caproic acid), arginine (1 amido, 4 guanidine valeric
acid), histidine, glycine (amidoacetic acid), alanine (amido propionic
acid), amido-valeric acid (amido-iso-caproic acid), liacine, pyrollidine
carboxylic acid, aspartic acid, glutamic acid (amido-glutaric acid),
phenyl-alanine, serine (hydroxy-amido propionic acid), purine
derivatives (_e.g._ guanine), indol derivatives (_e.g._ tryptophane
and skatol acetic acid), cystine (a thioserine anhydride),
glucosamine, and urea.

There are a few general reactions which are typical of all proteins, and
which can usually be traced to definite groupings in the molecule.
Amongst these is the biuret reaction: a pink colour obtained by adding a
trace of copper sulphate and an excess of caustic soda. This is caused
by the biuret, NH(CONH{2}){2} radical or by similar diacidamide
groups, _e.g._ malonamide, oxamide, glycine amide. Another general
reaction is with "Millon's reagent," a solution of mercuric nitrate
containing nitrous fumes. On warming the proteid with this reagent, a
curdy pink precipitate or a red colour is obtained. This reaction is
caused by the tyrosine group (p. oxy [alpha] amido phenyl-propionic
acid). Another general reaction is to boil the protein with 1:2 nitric
acid for some days. A yellow flocculent precipitate of "xanthoproteic
acid" is obtained, and this dissolves in ammonia and caustic alkalies
with a brown or orange-red colour. Another characteristic of proteins is
that on dry distillation they yield mixtures of pyridine C{5}H{5}N,
pyrrol C{4}H{5}N, and their derivatives.

On the subdivision, classification and nomenclature of the proteins much
ink has been spilled, and it is impossible in this volume to go into the
various systems which have been suggested. It should be noted, however,
that some writers habitually use the terms "proteid" or "albuminoid" as
synonyms for protein. The classification of proteins adopted in this
work is used because it is the most suitable for a volume on industrial
chemistry and has the additional merits that it is simple and is already
used in several standard works on industrial chemistry. It is based upon
the behaviour of the proteins towards water, a matter of obvious moment
in manufacturing processes. On this basis proteins may be divided into
albumins, keratins and gelatins.

Cold water dissolves the albumins, does not affect the keratins, and
only swells the gelatins. The behaviour in hot water confirms and
elaborates the classification. When heated in water, the albumins
coagulate at temperatures of 70°-75° C., the gelatins (if swollen)
dissolve readily, whilst the keratins only dissolve at temperatures
above 100° C. Albumins and keratins may be distinguished also from
gelatins by adding acetic acid and potassium ferrocyanide to their
aqueous solutions. Albumins and keratins give a precipitate, gelatins do
not. Another distinguishing reaction is to boil with alcohol, wash with
ether, and heat with hydrochloric acid (S.G. 1.2). Albumins give a
violet colour, keratins and gelatins do not.

=Albumins= may be first discussed. They are typified by the casein of
milk and by white of egg. Their solutions in water are faintly
alkaline, optically active, and lævorotatory. They are coagulated by
heat and also by mineral acids, alcohol, and by many poisons. The
temperature of coagulation (usually about 72° C.) is affected by
mineral salts, the effect being in lyotrope order (see Part V.,
Section I.). The coagulated albumin behaves in most respects like a
keratin. Some of the albumins (globulins) are, strictly speaking, not
soluble in cold water, but readily dissolve in weak solutions of salt.
The albumins are coagulated from these solutions, as usual, when
heated. Into this special class fall myosin (of the muscles),
fibrinogen (of the blood) and vitellin (of egg yolk). By a gentle or
limited hydrolysis of the albumins with dilute acids in the cold, a
group of compounds called albuminates are obtained. They dissolve in
either acids or alkalies, and are precipitated by exact
neutralization. They may also be "salted" out by adding sodium
chloride or magnesium sulphate. They are not coagulated by heat. After
further hydrolysis with either acids, alkalies or ferments, very
soluble compounds are obtained called albumin peptones or albumoses.
These are soluble in alkalies, acids and water, and are readily
hydrolyzed further into amido acids and acid amides. They are very
similar to the peptones obtained from keratins and gelatins. They are
not coagulated by heat.

=Keratins= are typified by the hair of animals. They soften somewhat
in cold water and even more in hot water, but are not dissolved until
digested for some time at temperatures exceeding 100° C. With some
keratins, however, the cystine group is to some extent easily split
off by warm water, and on boiling with water hydrogen sulphide is
evolved. The sulphur content of keratins is often greater than the
average for proteids. All keratins are dissolved with great readiness
by solutions containing sulphydrates and hydrates, _e.g._ a solution
of sodium sulphide. In solutions of the hydrates of the alkali and
alkaline earth metals, keratins behave differently. Some dissolve with
great ease, some with difficulty, some only on heating and some not
even if digested with hot caustic soda. They are dissolved (with
hydrolysis) by heating with mineral acids, yielding peptones and
eventually amido acids, acid amides, etc. Many keratins have a
comparatively low content of nitrogen.

=Gelatins= are very difficult to distinguish from one another, their
behaviour being closely similar to reagents. They are also very
readily hydrolyzed even with water, and the products of hydrolysis are
even more similar. The gelatins are known together, commercially,
under the general name of gelatine. Gelatins of different origin,
however, have undoubtedly a different composition, the nitrogen
content being variable. If the gelatins are not bleached whilst they
are being manufactured into commercial gelatine, they are called
"glue." Gelatine is colourless, transparent, devoid of taste and
smell. It is usually brittle. Its S.G. is about 1.42, and it melts at
140° C. and decomposes. It is insoluble in organic solvents. When
swelling in cold water it may absorb up to 12 times its own weight of
water. The swollen product is called a "jelly." Jellies easily melt on
heating and a colloidal solution of gelatine is obtained. This "sets"
again to a jelly on cooling, even if only 1 per cent. gelatin (or
less) be present. The solution is optically active and lævorotatory,
but with very variable specific rotation. Some observers have thought
that the different gelatins have different specific rotations and may
so be distinguished. Gelatins are precipitated from solutions by many
reagents, such as alcohol, formalin, quinone, metaphosphoric acid,
tannins, and many salt solutions, _e.g._ those of aluminium, chromium
and iron, and of mercuric chloride, zinc sulphate, ammonium sulphate,
potassium carbonate, acidified brine. Many of these precipitations
have analogies in leather manufacture (see Parts I. to IV.). The
gelatin peptones or gelatoses are formed by hydrolysis with acids,
alkalies, ferment or even by digestion with hot water only. A more
detailed description of the properties of gelatine is given in Part
V., Section I. Gelatine is sometimes called "glutin" and "ossein."

Animals are much the most important source of proteins, especially of
those which are of importance in industrial chemistry. Proteins occur
in nearly every part of all animals, and the "protoplasm" of the
living cell is itself a protein. The keratins include the horny
tissues of animals: the epidermis proper, the hair, horns, hoofs,
nails, claws, the sebaceous and sudoriferous glands and ducts, and
also the elastic fibres. The gelatins are obtained from the collagen
of the skin fibres, the bones, tendons, ligaments, cartilages, etc.
Fish bladders yield a strong gelatin. The albumins are obtained from
the ova, blood, lymph, muscles and other internal organs of animals.

The classification of proteins herein adopted fits in well with the
scope and purpose of this volume. The keratins are of little
importance in chemical industry, but are of immense importance in
mechanical industry, _e.g._ the woollen trade, which is based upon the
keratin comprised by sheep wool. The collagen of the hide and skin
fibres is of vast importance to chemical industry, and is the basis of
the extensive leather trades discussed in Parts I. to IV. The waste
pieces of these trades, together with bones, form the raw material of
the manufacture of gelatin and glue, as discussed in Part V. The
proteids of animals' flesh and blood, milk and eggs form the source of
the food proteins discussed in Part VI. The food proteins embrace
chiefly albumins, but gelatins and even keratins are involved to some
extent.

PART I.--HIDES FOR HEAVY LEATHERS

Section I.--THE RAW MATERIAL OF HEAVY LEATHERS

The term "hide" possesses several shades of meaning. In its widest sense
it applies to the external covering of all animals, and is sometimes
used derogatively for human skin. In this wide sense, it is almost
synonymous with the term "skin." The term "hide," however, has a
narrower meaning, in which it applies only to the outer covering of the
larger animals, and in this sense is used rather in contrast with the
term "skin." Thus we speak of horse hides, cow hides, camel hides, and
buffalo hides. It is used in this sense in the title of Part I. of this
volume. As such hides are from large animals, the leather which is
manufactured therefrom is thick and in large pieces, and is therefore
commercially designated as "heavy leather." From the standpoint of
chemical industry hides are amongst the most important of animal
proteins, and their transformation into leather for boots, shoes,
belting, straps, harness, and bags comprises the "heavy leather trade,"
which is one of the largest and most vital industries of the country.
The heavy leather trade predominates over other branches of leather
manufacture, not only because of the comparatively large weight and
value of the material handled, but also because the resulting products
have a more essential utility. There is also a still narrower use of the
term "hide," in which it applies only to the domesticated cattle--the
ox, heifer, bull and cow--which use arises from the fact that the hides
of these are both the largest and most valuable portion of the raw
material of the heavy leather industries. In a very narrow sense the
term is also sometimes applied only to ox hides, which for most heavy
leathers are the ideal raw material.

=The Home Supply= of hides forms a large important proportion of
the total raw material. Its importance, moreover, is rapidly increasing,
for the excellence and abundance of the home supply determines the
extent to which it is necessary for the industry to purchase its raw
material abroad. The position of our national finances makes this an
increasingly serious matter, for hides are comparatively a very
expensive material.

The quality of our home supply of hides is very valuable, being
determined by the conditions of the animal's life, its precise breed,
and by other factors such as age and sex. The best hides are usually
obtained from animals which have been most exposed to extremes of wind
and cold, as such conditions tend naturally to develop a thicker and
more compact covering. Broadly speaking, these include the hides from
cattle of the northern and hilly districts. The age of the animal when
killed is also a dominating factor. Calf skins are very soft, fine
grained and compact, the state of rapid growth favouring the existence
of much interfibrillar substance. The youngest animals supply suitable
raw material for various light leathers (see Part II., Section V.), and
are also very suitable for chrome work (see Part III., Section III.).
Bull and cow hides, on the other hand, are from animals whose growth is
complete, and show in consequence a lack of interfibrillar substance,
coarse fibres and a rough and often wrinkled grain. The resulting
leather tends consequently to be spongy, thin, empty and non-waterproof.
Intermediate between these extremes are the hides of the ox and heifer,
large, yet of good texture, and well supplied with interfibrillar
substance. These hides are much the best for sole leather, a firm,
smooth-grained and well-filled leather being needed. The term "kip" is
often applied to small hides and to hides from large calves. In the
trade, however, "kip" is sometimes used also for larger hides, as a
verbal enhancement of value; just as a man with a few old fowls is said
to keep "chickens." Cow hides tend to be "spready," _i.e._ to have a
large area per unit weight, and are therefore more suitable for dressing
leather. Bull hides are thicker in the neck and belly, and thinner in
the back, which characteristics reduce their commercial value.

Market hides are sold by weight, and are therefore classified chiefly by
their weight, which is marked on near the tail by a system of
knife-cuts. The animals are flayed after cutting the hide down the belly
and on the inside of the legs.

Of the various breeds, "Shorthorns" yield a large supply of useful
hides. The name, however, covers a variety of similar breeds, and the
hides therefrom are rather variable in texture and quality. They tend to
be greasy owing to high feeding. The "Herefords," obtained from Midland
markets, are generally excellent hides for sole and harness leathers.
They give a good yield of butt pelt, a stout and smooth shoulder, and
are not often greasy. "Devons" yield a good-textured and well-grown
hide, but are often badly warbled. The "Sussex" cross breeds yield
somewhat larger hides. "Suffolk Red Polls," common in East Anglia, yield
a good butt, and the cow hides make good dressing leather. "Channel
Island" cattle yield very thin hides, but with a fine undamaged grain.
Scotch hides possess deservedly the very highest reputation. The
climatic conditions favour the production of a hardy race of cattle with
thick well-grown hides, yielding a large proportion of butt. These hides
are amongst the best obtainable for heavy leather, and particularly for
sole leather. "Highlanders," "Aberdeen Angus," "Galloways" are typical
breeds, with short neck, legs and straight backs. Cross breeds are also
excellent (_e.g._ "Scotch Shorthorns"). The natural value of these hides
is further enhanced by the usual care in flaying. "Ayrshires" yield good
milch cows and consequently yield often a more spready hide. The Welsh
breeds for rather similar reasons also yield valuable hides. The Irish
"Kerrys" are small but stout, and yield hides suitable for light sole
leather. Irish cross-breeds, Shorthorns, have a rather bad reputation,
and are often ill flayed.

All the varieties of the home supply are subject to various defects,
which influence seriously their commercial value. One of these defects
is warble holes or marks, caused by the Ox Warble fly (_Hypoderma
bovis_). This is a two-winged fly about half an inch long. The larva of
this fly, the "Warble maggot," lives and thrives in the skin of cattle,
and causes a sore and swelling. The life-history of this insect is still
in dispute, but it is generally thought that the eggs are laid in the
hair on the animal's back, and the young larva eats its way through the
hide until just below the dermis, and there feeds until mature. It then
creeps out of this "warble hole," falls to the ground, pupates for a
month, after which the imago or perfect insect emerges from the
chrysalis. Hides which have been thus infected have, in consequence,
often quite a number of holes through the most valuable part of the
hide, thereby rendering it unsuitable for many kinds of leather. Even
old "warbles" which have more or less healed up are a weakness, and
warbled hides and leather fetch a decidedly lower price than undamaged.
Another of these defects is bad flaying. Clearly the hide should be as
little cut as possible, but many of our market hides are abominably
gashed and often cut right through. This, of course, often reduces
seriously the commercial value of the hide. Careless treatment after
flaying also results in another common defect, viz. taint. As the term
implies, the hide is partly putrefied, sometimes only in patches, but
sometimes also so extensively as to render the hide quite rotten and
quite incapable of being made into leather at all. Hides are of course
putrescible, and dirt, blood, dung and warm weather encourage rapid
putrefaction. As market hides are usually uncured, this defect is
constantly appearing, and is a cause of considerable loss. Other defects
are due to injuries to the animal before it is killed, _e.g._ brands,
scratches due to hedges and barbed wire, old scabs, goad and tar marks.
All these reduce the value of the hide.

All the defects in hides involve a very serious loss to the community,
and the time is rapidly approaching when their continuance is
insufferable. The loss is not usually very considerable to any
individual, though very large in the aggregate. The hide is a minor part
of the beast's value, and a somewhat damaged hide does not involve a
very serious loss to the farmer. Some with typical stupidity regard a
few warbles as "the sign of a healthy beast." These defects involve
practically no loss to the hide merchant, tanner or currier, as each
pays less for damaged material. The loss falls upon the community, and
the time is ripe for the community to insist upon the elimination of
these defects. The national resources will be for some years strained to
their uttermost, and preventable damage must be considered intolerable.
The principal defects in hides are preventable, and ought to be
prevented. The warble fly could, by a united effort, be rendered before
long practically extinct, a task which is facilitated by the fact that
it is not migrative. Bad flaying and careless treatment of hides
resulting in putrefaction are still more easily remedied. The communal
slaughter-house is long overdue from the standpoint of public health,
and would, under conditions of cleanliness and skilled workmanship and
oversight, also solve the problem of ill-flayed and tainted hides.

The question of the raw material is of first importance to the leather
trades. There was, before the commencement of the European War, a
steadily increasing scarcity of hides, causing a constant increase in
their price. This was due partly to the fact that cattle were increasing
at a less rate than the population, partly to the growth of
civilization, and more extensive use of leather in proportion to the
world's population, and partly to the constant discovery of new uses for
leather, _e.g._ for motor cars, aeronautics, etc. The question of raw
material was under these conditions serious enough. The terrific
slaughter, necessary at the same time to provide the belligerents with
food and the army with leather, is bound to result in a serious crisis
for the leather industries; and in conjunction with the country's
financial condition, will make it absolutely necessary that all care
should be taken with the raw material of one of our most important
industries. The farmer who pays no heed to the warble fly, the man who
gashes the hide in flaying and who allows the hide to putrefy, are
equally criminal with the man who throws bread crusts into the dustbin.

It is impossible to foresee, as yet, anything in the nature of a
satisfactory solution to the problem of raw material, especially in
respect to heavy leather production, for the food question will rank
first in the popular mind, and the earlier slaughter enjoined for the
more economical production of meat will scarcely tend to increase the
proportion of heavy hides.

=The Foreign Supply= of hides is also of great importance and value. In
the case of imported hides precautions to prevent putrefaction are
essential, and some method of "curing" is always used.

=Salting= the hides is one of the most satisfactory methods for
temporary preservation. The action of salt is hygroscopic, and mildly
antiseptic. Moisture is withdrawn from the hides, which are then under
conditions no longer favouring the growth of bacteria. Well-salted
hides will keep for years, especially if quite clean. A light salting
is also useful for a short preservation, and is becoming common in
hide markets and tanneries during the summer and autumn months.
Salting is a method used extensively in the United States. The "packer
hides" of the stockyards are carefully and systematically salted with
about 25 per cent. of salt and stored in cool cellars. The hides are
so piled up in heaps, that brine easily drains away. The great
disadvantage of salting is the so-called "salt stains." These stains
have been ascribed to the iron in the salt, to the iron in the blood,
to calcium sulphate in the salt, and also to chromogenic bacteria,
whose development is favoured by salting. The relative importance of
these factors is not yet satisfactorily determined, but cleanliness
and pure salt tend to eliminate the trouble.

=Drying= the hides is a less satisfactory cure. The principle is
similar, viz. removal of moisture. Dried hides are, however, much
drier than salted, and are quite hard and horny, hence the name "flint
hides." The hides also lose much weight, a considerable advantage in
reducing freight. Tropical hides are often flint-dry, and where
preservatives are expensive or unprocurable, it is often the only
practicable method of cure. Nevertheless, the method has many serious
disadvantages, and is difficult to execute. If dried too slowly the
hides putrefy partially; if too quickly they dry on the outside, and
the interior is left to putrefy. The fact that hides are of uneven
thickness, and the climate often hot, increases the difficulty, and
often results in partial destruction of the fibrous structure of the
hide. When dried, moreover, the hides are still subject to the attacks
of insect larvæ, for the prevention of which the usual sprinkling of
naphthalene or arsenic is only an imperfect remedy. This method of
cure is also a nuisance to the tanner, who has to employ labour, pits
and time in attempting to restore the hides to their original
condition, and often loses up to ten per cent. of the goods in so
doing. Dried hides are also subject to the presence of anthrax.

=Dry Salting= the hides is an excellent method of curing. As the name
implies, it combines methods of drying and salting which are used
alternatively. The method is used extensively in South America. A
modified form of it is also used for preserving the "E.I. kips," which
are cured, however, not with common salt, but with earth containing up
to 70 per cent. of sodium sulphate. Dry-salted hides are largely free
from the defects of dried hides, but of course are more trouble to the
tanner in the process of soaking (see Section II.) than the wet-salted
goods.

=Freezing= the hides is now a commercial process. On the whole the
process is satisfactory, but the expansion of water after freezing may
tend to damage the hide fibres.

Sterilizing the hides has been frequently suggested, but no method has
yet been advocated which does not interfere either with the tanning
processes or with the quality of the finished leather.

Hides from the European Continent, usually wet salted and well flayed,
exhibit much the same variable quality as the home supply, those from
highland districts tending to be thick, yet even, well grown, tight
textured and smooth grained, whilst those from lowland regions are
less satisfactory. Thus hides from the Swiss Alps and Scandinavia have
ranked high, whilst the spready Dutch cows are typical of a lowland
hide. In the hides which once came from Germany the same features
appear. Bavarian highland hides had an excellent reputation, whilst
those from Berlin, Cologne, etc., tended to be long in shank and not
well grown. French hides are often ill flayed, and Spanish and
Portuguese are often subject to scratches. Italian hides have a very
good name, being small but stout in butt.

The American supply is important. South America yields an excellent
class of hide, salted or dry-salted. They are from an excellent breed
of animals, slaughtered and flayed with every care, and efficiently
cured. A most serious defect in this class of hide is the "brand,"
which is both deep and large and in the most valuable part of the
hide. One side, however, is usually unbranded, so that each hide
yields one good "bend." These hides, _e.g._ "Frigorifics," have
recently been much more extensively tanned in Britain because of the
shortage in the home supply of market hides caused by the European
War. South America also yields good horse hides. North American hides
are usually wet-salted (_e.g._ packer hides). They are usually good.
Central America yields mostly dried hides exhibiting usual defects.

The Asiatic supply comprises the frozen China hides, which are clean
but small, with flaying of uncertain quality. There are the buffalo
hides from Asia and East Europe, which are suitable for cheap and sole
and strap leather, and also the dry-salted "E.I. kips," obtained from
a small breed of Indian cattle, and extensively made into upper
leather. The Asiatic humped cattle also provide a limited supply. The
African supply is of increasing importance. The tropical parts yield
dried hides of uncertain quality, but the more temperate parts of
South Africa yield a growing supply of good quality.

REFERENCES.

"The Manufacture of Leather" (Bennett), pp. 27-37.

"Principles of Leather Manufacture" (Procter), pp. 33-56.

"The Ox Warble or Bot Fly" (E. Ormerod).

"The Making of Leather" (Procter), pp. 2-22.

Section II.--THE PREPARATION OF PELT

Before hides are tanned it is necessary for them to pass through a
series of preparatory processes. The object of these processes is to
obtain from the hide the true hide substance in a pure and suitable
condition. Each class of leather has its own appropriate processes, the
adjustment of which largely determines the quality of the finished
article. So prominent is the influence of these preparatory methods that
the paradox "good leather is made before tanning" is in trade circles
almost a platitude. These processes, sometimes lumped together under the
general name of "Wetwork," comprise soaking, liming, beam house work and
deliming. These will be discussed in turn.

The term applied to the hide after these processes, but before tannage,
is "pelt."

=Soaking= has for its object the cleansing and softening of the hides,
chiefly by means of water. It aims at the removal of dirt, blood, dung,
and curing materials by washing. The process is usually simple, and is
much the same for all classes of leather. The ideal to be aimed at is to
restore the hide to its condition when it left the animal's back.
Cleanliness in leather manufacture is as essential at the commencement
as anywhere, for the hide is in its most putrescible state. The soluble
proteids (blood, lymph, part of dung, etc.) which always adhere to hides
encourage the rapid growth of putrefactive bacteria, and cannot be
washed away too soon. Dung is often difficult to remove, being caked on
the butt end amongst the hair. Soaking only softens it, and mechanical
removal is usually necessary. If such substances are not removed, they
go forward with the goods into the lime liquors, causing stains,
loss of hide substance, and counteracting plumping.

The detailed method and time of soaking are determined mainly by the
nature of the cure. One of the purposes of the soak liquors is to
dissolve the salt used in curing hides and to rehydrate the hide and
make it again soft and pliable. As a 10-per-cent. salt solution exerts a
solvent effect on hide substance, it is necessary soon to change the
first soak liquor of salted goods.

Market hides, which are uncured, require the least soaking, the
cleansing effect being most needed. The hides are inserted into pits
("water dykes") of water for a few hours, and the water changed once or
twice. The soaking should not be prolonged as the hides are so
putrescible, and where it is customary to leave the goods in a soak
liquor overnight, it is advantageous to add a little slaked lime to the
water before inserting the goods. This not only softens hard water, but
is mildly antiseptic and plumping, and forms a suitable introduction to
the liming proper. Each pit contains a "pack" of 30-50 hides, according
to its capacity, which varies in different tanneries from 1000 to 2000
gallons. Tainted goods, which are indicated by a characteristic white
colour on the flesh side and by loose hair, need a preliminary washing
either in a "drum," "tumbler" or in a "paddle." This ensures a rapid
change of liquor and the removal of most of the putrefactive agencies.
Bad cases may need the application of antiseptics, such as immersion in
0.1 per cent. carbolic acid; but if possible these should be avoided, as
they lengthen the time required for liming. After drumming or paddling,
tainted goods should be placed directly into a lime liquor.

Salted hides need very similar treatment to uncured hides, but the
soaking is longer, because of the dehydration caused by salting. Hence
they receive also a greater number of changes of water, three or four
usually, but often more. As much loose salt as possible should be shaken
from the hides before insertion into any liquor. The employment of drum
or paddle before pit soaking is extremely useful to effect the rapid
removal of superficial salt, and is also useful after pit soaking to
remove the last traces.

Dried and dry-salted goods need a soaking still more prolonged, up to
one week if water alone be used. With the assistance of caustic soda,
however, the process can be shortened to about two days. The first soak
liquor should consist of a 0.1 per cent. solution of caustic soda, and
after the goods have been inserted twenty-four hours, they will be
materially improved by a few hours' drumming or paddling. Another
caustic soda soak will complete the process. Sodium sulphide crystals
may replace caustic soda, but about three times the weight will be
needed. Carbonate of soda and caustic lime also are a convenient
commercial substitute for caustic soda. For 10 lbs. caustic soda, use 36
lbs. carbonate and 7 lbs. lime. Extra lime should be added in all cases
when the water is hard. Acid liquors will also soften dried and
dry-salted goods, but such processes do not fit in so well with the
subsequent liming. The use of putrid soaks and stocks may be now
considered out of date.

=Liming= follows soaking, and consists essentially in immersing the
hides for 7-10 days in milk of lime. The chief object in view is to
loosen the hair and prepare for its mechanical removal. Liming takes
place in pits, the tops of which are level with the limeyard floor.
The lime is slaked completely and mixed well with water in the pit,
being particularly well plunged just before the insertion of a pack of
goods. Saturated limewater is only a 0.13-per-cent. solution. The
goods are occasionally "handled" _i.e._ hauled out of the pit and
reinserted after plunging ("hauling" and "setting"). This is necessary
to keep the liquor saturated with lime. The hides are inserted one by
one, each being "poked down" to ensure its contact with the liquor.
The goods are invariably immersed first in a previously used lime
liquor. Most tanneries now carry this out in a systematic way, so as
to ensure regularity in the process. As the goods are large and heavy
it is less laborious to carry out the whole process in one pit. In
this "one-pit system" the goods are inserted for (say) four days in an
old used lime liquor, with occasional handling; this liquor is then
run to the drain and a new liquor made up in the same pit, into which
the goods are inserted for (say) five days. They are then hauled and
sent to the unhairers. Each pack thus gets two liquors, old and new.

A better method is the "three-pit system." In this case each pack
receives three liquors and has (say) three days in each, first an "old
lime," then a "medium lime," and finally a "new lime." This system
ensures a greater regularity of treatment, and is deservedly the most
popular method for liming hides for sole leather. After being used once
as a "new lime," a liquor then becomes a "medium lime," and after being
thus used becomes the "old lime" which receives the green hides from the
soaks. The system involves the goods being shifted twice to another pit,
which is more laborious than reinsertion into the old pit, but if the
limeyard be arranged in "sets" or "rounds" of three pits, the shift is
usually only to the adjacent pit. One special advantage of this system
is that the top hides in one pit become the bottom hides in the next
pit, and _vice versâ_. Rounds of more than three pits are sometimes
used.

Many factories have now adopted systems in which there is no handling at
all. The hides are suspended in lime liquors which are agitated by
mechanical contrivances (_e.g._ Tilston-Melbourne process), or by jets
of compressed air (_e.g._ Forsare process). The goods are soaked and
limed "mellow to fresh" by changing the liquors by means of pumps, air
ejectors, etc. Thus the hides need no labour from first being inserted
until drawn for depilation.

In liming, the whole of the epidermis as well as the hair is loosened,
and is subsequently removed in depilation. The corium or true hide
substance becomes much more swollen by imbibation of water, and when
taken out of the new lime is "plumped" to very firm jelly. This plumping
is a matter of prime importance to the tanner. The coarser fibres are
thereby split up into the finer constituent fibrils, which fact assists
very materially in obtaining a quick and complete tannage, good weight,
and a firm leather. During the liming, the natural grease of the hide is
saponified or emulsified, which prepares for its removal in scudding.
Liming is thus a complex process: the hair is loosened, the hide is
plumped, and the grease is "killed." All these results may be hastened
by the use of other alkalies in addition, and most heavy leather yards
assist the liming by adding also sodium sulphide or caustic soda or
both. Sodium sulphide is a powerful depilatant, and will alone unhair
hides easily in strong solutions even in a few hours. As in solution it
forms caustic soda by hydrolysis, it possesses also the powerful
plumping and saponifying powers characteristic of the latter. The
addition of arsenic sulphide (As{2}S{2}) (realgar) to the lime when
slaking causes the presence of calcium sulphydrate in the lime liquors
thus made. This is also a powerful depilatant, but not much used for
heavy leather.

The function of the lime in depilating is complex and has occasioned
much discussion. Its main purpose, however, is that of a partial
antiseptic. When hides putrefy, one of the first results is that the
hair is loosened. In America depilation by "sweating" is carried out
commercially by such a mild putrefaction, the lime liquor permits a
similar fermentation at a slower rate, and all tannery lime liquors are
swarming with putrefactive bacteria. Liming is thus a safer method than
sweating, which may be easily carried too far. Various workers have
isolated specific organisms--Wood a _bacillus_, Schmitz-Dumont a
_streptococcus_--but it seems highly probable that the limeyard bacteria
are just the common organisms of putrefaction sorted out or selected by
the exact nature of the liquor and the method of working the limes. Many
putrefactive bacteria are very adaptable and could easily accommodate
themselves in this way. It is known that the exact nature of the
culture medium has a great influence on the rate of development of such
organisms, and which particular species thrive and obtain predominance
in any limeyard will depend upon the amount and nature of the dissolved
organic matter available as food, and upon the exact alkalinity and the
concentration of other apparently inert substances, such as common salt
and sodium, calcium and arsenic salts. Hence no two lime liquors operate
alike, and approximate regularity is only assured by systematic method.
In handling and shifting, the organisms are subjected to further
selection, and the most adaptable survive. It is probable that different
species may act symbiotically. The depilating organisms of lime liquors
are probably mostly anærobes, but some may be anærobic by adaptation. It
is probable that ærobic ferments commence the depilation, but this will
be done before the goods are put into work, or at any rate before they
reach the limes. More strictly, it is the enzymes secreted by bacteria
which are directly responsible for the hydrolytic work; these enzymes
are chiefly proteolytic (proteid splitting), but the lipolytic (fat
splitting) enzymes have also a place.

The lime, however, not only limits and selects the course of the
putrefaction, but also affords more positive assistance. Lime plays its
own hydrolytic part and assists the depilation by purely chemical
action. Lime will unhair without the assistance of bacteria, but its
action is slow and forms a minor part of the operation in the average
limeyard. This action is due chiefly to its progressive formation of
calcium sulphydrate from the cystine group of the softer keratins. Lime
also plays an essential part in assisting the putrefactive fermentation.
It softens the keratins and thus assists the bacterial attack, it
hydrolyzes other proteids and provides the bacteria with food in
solution, the calcium ion increases the proteolytic action of certain
enzymes, and finally the apparently inert excess of undissolved lime has
an accelerating effect on the bacterial activity.

In the average limeyard these various functions are inextricably mixed
up, and it is impossible to assign any definite proportion of the total
depilatory effect to any of the factors at work. Lime alone will unhair,
bacteria alone will unhair, and sulphides will also unhair without lime
or bacteria, but in the limeyard all three agencies are at work.
Putrefactive fermentation, however, obtains a good start. Ærobic
fermentation commences with the slaughter of the animal, and the
anærobic organisms soon commence their part, and are at work in the hide
house and soaks. On entering the limes, the purely chemical hydrolytic
action of lime is added to that of the bacterial enzymes as well as the
action of lime as bacterial assistant, and the three continue to operate
side by side. Each gives rise to the formation of calcium sulphydrate,
whose own special solvent effect is superadded. If sulphydrates be
deliberately added to the liquors there is yet another factor assisting.
Speaking broadly, the bacterial enzymes have their maximum activity in
the old limes, and the chemical action of sulphydrate formed from the
keratin cystine is also at a maximum in these liquors. The chemical
action of added sulphide, and the simple hydrolytic action of calcium
hydrate have their maximum activity in the new limes. Most observers
would agree that in practice the bacteria shoulder the greater part of
the work.

From the limeyard is taken about the only waste bye-products of the
tannery, viz. the residues from the soak and lime pits. These consist
mainly of lime and chalk, with some hair and dung, and possibly a little
sulphide. The sludge possesses some value as a manure, especially if
from the soak pits on account of the greater nitrogen content. (Part
VI., Section I.)

=The Beam House Work= consists in the mechanical removal of those
parts of the hide not wanted for leather manufacture. _Unhairing_
removes the hair and the epidermis made loose in liming. The hides are
placed over a sloping "beam" with a convex surface, and the hair scraped
off with a blunt concave and double-handled knife. The hides are then
thrown into a pit of water. The hair is carefully collected, washed well
with water, preferably centrifuged, and then dried out by a current of
warm air. It forms a valuable bye-product. White hair is usually kept
separate and fetches a higher price. _Fleshing_ is the next process. The
hides are again placed over a beam, with the flesh side (_i.e._ the side
nearest the flesh) uppermost. Skilled workmen then cut off, with a sharp
convex knife, the fat, flesh and connective tissue left in flaying.
_Rounding_ is usually the next process. The unhaired and fleshed hide is
spread out flat and cut up into butt, shoulder and a pair of bellies.
These parts have different commercial values, and may afterwards be
tanned by different methods for very different purposes--for dressing
leather, and sometimes even for sole leather. _Scudding_ is the last
piece of beam work. The fleshed hides (whether rounded or not) are
washed, or at least rinsed, with water, and again placed on the beam
grain side up. They are then scraped with a rather sharp concave knife,
to remove "scud," which consists of hair roots and sheaths, lime soaps,
fat, pigment and other dirt. Short hair is shaved off by a very sharp
hand knife.

The beam work demands a certain amount of skill from the workmen,
especially from the flesher, whose sharp knife may prove very wasteful
in incompetent hands. Hand labour was slowly but surely being replaced
by machinery before the war, and war-time conditions have greatly
accelerated the rate of transition. Beam house machinery is rapidly
becoming universal. The machines are cumbrous and expensive in cost and
in power, but machine work is quicker, less laborious, and needs much
fewer workmen. Many types of machine have been suggested, but the most
useful are those in which the hides pass over rollers and are
simultaneously acted upon by a rapidly revolving cylindrical knife with
spiral blades, one half being a left-handed and the other a right-handed
spiral, so that the hide is scraped outwards as well as in the direction
of motion. The part of the hide being acted upon rests on a pneumatic
roller. By changing the type of spiral knife cylinder the machine will
unhair, flesh or scud.

=Deliming= is a general name covering a number of similar operations
whose primary object is the neutralization and removal of the caustic
lime and soda in the plumped pelt, or at any rate on the surface of the
hide. This is a preparation for the tan liquors. All the tannins and
many associated substances darken rapidly with oxidation when in
alkaline solution, so that to place the fully limed hide in a tan liquor
would give a dark-coloured leather. A short insertion in a bath of weak
acid would secure the elimination of surface lime and the disappearance
of this difficulty, but there are other purposes in deliming. The more
completely lime is removed the more the plumped pelt "falls" into a
soft, pliable, unswollen and relaxed condition, and this change assists
very materially in the production of a soft dressing leather, suitable
for boot uppers, bags, etc. For such leathers, therefore, the deliming
must be much more complete than for sole leather, in which the object is
to obtain a firm and plump leather.

In the case of the softer dressing leathers, experience indicates the
advisability of allowing some further bacterial action on the
interfibrillar substance in order to produce the requisite pliability
and softness. This is secured by "bating" the hides. This process
consists in immersing the goods into a cold fermenting infusion of hen
or pigeon dung. The infusion is made in a special tub or pit with warm
water and allowed to stand for a day or two until the fermentation has
commenced, and then run into the bating pit through a coarse filter such
as sacking. The hides are immersed for some days, but are handled
frequently to ensure an even effect. The bate is always slightly
alkaline. The caustic alkalinity increases rapidly at first owing to the
diffusion of caustic lime, then at a slower rate, afterwards slowly
declining. This is explained by the production of organic acids, and
their salts with weak bases from the dung infusion by the action of
bacteria. The total alkalinity of the bate liquor increases rapidly at
first owing to the diffusion of lime and its liberation of organic
bases, then very slowly, but towards the end of the operation the total
alkalinity increases very rapidly indeed, owing probably to the
commencement of a violent anærobic fermentation which produces ammonia
and other organic bases, and which heralds the approach of a
putrefactive action, which if allowed to continue for even a short time
will ruin the hides. Bating is consequently a risky process, and needs
experienced oversight. For goods which need only a mild bating, there is
the alternative of giving a longer liming in older limes. This of course
involves more bacterial hydrolysis, and perhaps does it in a safer, more
economical and certainly in a less offensive manner. Bating is often
followed by a further deliming by acids. Boric, lactic, acetic, formic
and butyric acids are all used, and with care even hydrochloric and
sulphuric acids may be employed. Innumerable "artificial" bates have
been put on the market, but most are merely weak acids, acid salts or
salts of strong acids with weak bases. An American "bacterial bate"
consists of a lactic fermentation of glucose in the presence of glue.

Closely similar to bating is "puering," investigated by Wood.

Drenching is another fermentive deliming process. In this the goods are
inserted into an infusion of bran. This is made by scalding the bran
with hot water, and allowing it to stand until it is about 70°-90° F.
The infusion is then "inoculated" with a few gallons of old drench
liquor, and the goods are immersed. This fermentation has been examined
carefully by J. T. Wood. First the enzyme cerealin converts bran starch
into glucose, which is then fermented by the drench bacteria with the
production of lactic acid, some acetic acid and small amounts of formic
and butyric acids. The butyric fermentation is liable to become too
violent. These acids, as they are formed, neutralize the lime in the
hides and plump the pelt slightly.

Various gases (carbon dioxide, hydrogen, nitrogen, methane and
sulphuretted hydrogen) are involved, and the proportion produced in the
pelt itself has a peculiar opening effect on the hide fibres. The
activity of the drench can be decreased by dilution and by using a less
starchy bran, and can be increased by adding pea meal or rye meal.

Drenching usually follows bating. Scudding sometimes follows deliming.

The theory of the volume and elasticity changes of pelt during
preparation will be better understood after considering the behaviour of
gelatine gels. The determining factors are the _nett_
charge of hydroxyl ions on the disperse phase, resulting from ionic
adsorptions, and the lyotrope influence of dissolved substances on the
continuous phase.

In softening dried hides the swelling may be due to either influence,
but the latter tends to loss of hide substance and the production of
soft leather.

In liming, the nett adsorption of hydroxyl ions is the principal factor,
but the lyotrope influence of the alkali cations and of the impurities
is important. Plump pelts are those in which the contained water is in a
relatively greater average state of compression. Few substances can
assist plumping, but many can hinder it. In plumping all lyotrope
influence is objectionable, and "sharp" (pure) alkali solutions are
required. Mellow limes reduce elasticity and plumpness by lyotrope
influence.

In bating and puering the essential change is that before the process
the swelling is due chiefly to adsorption of hydroxyl ions, whereas
afterwards it is due chiefly to a composite lyotrope influence.

REFERENCES.

"Principles of Leather Manufacture," Procter, pp. 108-184.

"The Manufacture of Leather," Bennett, pp. 49-113.

"Lyotrope Influence and Adsorption in the Theory of Wetwork,"
Bennett, _J.S.L.T.C._, 1920, pp. 75-86.

"Analytical Examination of Bating," Bennett, _Leather Trades
Review_, 1911, p. 972, and 1912, p. 28.

"The Bating, Puering and Drenching of Skins," by J. T. Wood.

SECTION III.--VEGETABLE TANNAGE

All tannages have for their object the conversion of the readily
putrescible hide tissue of the corium (the pelt) into an
imputrescible, insoluble and permanent material called "leather"
which, possessing considerable strength and pliability, is capable of
application to a variety of useful purposes. The conditions necessary
for this transformation have been clearly stated by Procter.[1] For
the production of leather from pelt "it is not only necessary to dry
the fibres in a separate and non-adherent condition, but so to coat
them or alter their chemical character that they are no longer capable
of being swelled or rendered sticky by water." Whatever substance will
secure this permanent dehydration of the hide fibres in a separate
condition is called a "tanning material." The change from pelt to
leather is known as "tannage," the process is termed "tanning," and
those who undertake it are "tanners."

[Footnote 1: "Principles of Leather Manufacture," p. 184.]

In "vegetable tannage" the tanning materials are of vegetable origin,
and contain a group of organic compounds called "tannins" which are
extracted by the infusion of these materials with water. Pelt, when
immersed in these infusions, is converted into leather, rather slowly;
but a gelatin solution gives an immediate precipitate of "amorphous
leather," even if the tannin infusion be exceedingly dilute. The
tannins are aromatic compounds of phenolic character, and contain
carbon, hydrogen and oxygen only, but our knowledge of their chemical
constitution is exceedingly small owing to their instability and
colloid nature, which make impossible their preparation in a pure
state. They are all, however, derived from either catechol or
pyrogallol, and yield these substances if carefully heated to about
200° C. The tannins are soluble in water, alcohol, acetone, ethyl
acetate and acetic acid, but insoluble in benzene, chloroform, carbon
disulphide, petroleum ether,
dilute sulphuric acid and _pure_ ethyl ether. The aqueous infusions of
the tannins are in reality colloidal solutions; _i.e._ heterogeneous
systems of two phases. The systems are lyophile, or, more particularly,
hydrophile, _i.e._ there is an affinity between the two phases. As usual
with lyophile systems the two phases may be considered as both liquid,
and an aqueous infusion of tannin forms an emulsoid sol, which therefore
is subject to the phenomenon of adsorption. The tannins are all
precipitated by solutions of basic lead acetate and copper acetate, and
many of them with varying completeness by solutions of many other
metallic salts and hydroxides, of basic dyestuffs and of alkaloids. They
give dark colorations with ferric salts.

The tannins are widely distributed in plant-life, but only in a limited
number of cases do the plants contain sufficient tannin to render them
of commercial importance. Tannin is found in all parts of plants, but
usually in greatest amount in the bark or fruit. The tannins are
classified into "pyrogallol tans" and "catechol tans," according to the
parent phenol. This classification is confirmed by their chemical,
analytical and practical behaviour, and the vegetable tanning materials
may be classified into the same two groups, for, although even the same
plant contains both pyrogallol and catechol tans, it is usual to find in
any one part of the plant that one group is predominant.

=Pyrogallol tans=, which are oftenest obtained from fruit or leaves,
contain usually about 52 per cent. of carbon. Used alone they produce a
rather soft and porous leather. Associated with them--in many cases
probably as decomposition products--are certain other substances of
well-known properties and constitution. These substances are not only
typical of the group, but also form the most valuable clue to the
chemical constitution of the group and the key to their chemical
behaviour. One of these substances is gallic acid (3:4:5
trihydroxy-benzoic acid C{6}H{2}(OH){3}COOH), which possesses
properties very similar to the tannins, but does not precipitate gelatin
and will not itself make leather. Another of these substances is ellagic
acid C{14}H{6}O{8}, a double lactone of a
hexa-hydroxy-diphenyldicarboxylic acid. This is deposited as an
insoluble yellow powder from infusions of many pyrogallol tans, by
boiling with dilute acids only, allowing them to stand for a few days.
In practice the deposit is found as mud at the bottom of the tan pits,
and also upon the leather, to which it strongly adheres. It is
technically known as "bloom." It is insoluble in acids and cold alcohol,
but soluble in alkalies. It is a feeble dye-stuff. The pyrogallol tans
yield very different amounts of bloom. Other associated substances are
the sugars. In practice these sugars ferment to lactic, acetic, and
other acids which cause "sour" liquors. Such liquors plump the hides and
tend to give firm, thick leather. These acids also probably cause
increase of adsorption of tannin by the hide and therefore assist in
giving "good weight." Solutions of pyrogallol tans all give a blue-black
colour with a dilute solution of ferric alum. If a solution of sodium
arsenate be added to an infusion of pyrogallol tan diluted until no
longer distinctly coloured, and the mixture allowed to stand for about
two hours, a green colour develops at the surface of the liquid. The
reaction is due to gallic acid or a similar grouping, and is, in the
author's experience, the most satisfactory qualitative test for the
group. Another test is to mix equal volumes of a 0.4 per cent. infusion
of tan and a 10 per cent. solution of sodium bisulphite; a few drops of
10 per cent. potassium chromate are added, and either a transient
blood-red colour or a more permanent deep purple is obtained. The former
colour is due to gallic acid. If a tannin infusion be largely diluted
with hard water and a little iodine solution added, the pyrogallol tans
yield either a purple-red or a dark blue colour, the former being a
reaction of gallic acid. Pyrogallol tans yield no precipitate with
bromine water. They yield a yellow or brown colour when one drop of
infusion is added to concentrated sulphuric acid.

Myrabolans is one of the most important of the pyrogallol tanning
materials. It is a name given to the dried fruit of _Terminalia chebula_
and other species of Indian trees. The nuts resemble an elongated
walnut. They are dried and exported from many parts of India to all
parts of the world, but largely to this country. The varieties of
commerce are named according to origin and quality: thus we have "J1's,"
_i.e._ Jubbelpore, No. 1 quality, "R1's" (Rajpore, No. 1),
"B1's" (Bhimley, No. 1), etc. The little difference in tannin strength
(about 32 per cent.) in these varieties is usually compensated by
corresponding differences in price. The quality of myrabolans cannot be
safely judged by appearance. Much bloom is deposited by myrabolans
liquors, especially by "J's." Myrabolans are amongst the most sugary of
tanning materials, containing up to 5-1/2 per cent. It is therefore one
of the best materials for giving a plump leather. Broadly speaking,
those varieties which yield most sugar yield least bloom, and _vice
versâ_. Myrabolans tannin has a small affinity for hide substance and
penetrates the hide very slowly. It gives a "mellow" tannage, but a
bright, good colour, which characteristics are imparted to the leather
when the material is blended with other materials containing dark or
astringent tannins. When used alone it yields a rather spongy leather,
and it is not considered a good weight-giving material, though its
acid-producing powers are very helpful to other more astringent tannins.

Valonia has been the other staple tanning material of the heavy leather
trade. It is the acorn cup of oaks common in Asia Minor and Greece,
chiefly the Turkish oak (_Quercus ægilops_). The fruit is gathered when
ripe and dried in layers of about one foot deep until the acorn drops
out, Smyrna is the great export centre. Greek valonia is obtained from
many parts of the Archipelago and mainland. It is gathered in a more
immature condition and includes the acorn. It is considered slightly
inferior in strength and colour to the Smyrna valonia. The exterior of
the acorn cup is covered with rather scaly protuberances known as
"beard," which contains usually about 40 per cent. of tannin. The cup
alone contains usually about 25 per cent. tannin, and the whole about 30
per cent. The valonia tannin has been thought to contain two chemical
individuals, only one of which produces bloom. Parker and Leach[2] found
that the tannin of the cup produces more bloom than that of the beard,
and that Smyrna valonia yields more bloom than Greek. The more bloom is
deposited, the less acid will be produced. Under all conditions the
yield of bloom is large, and its deposition in and on the leather
assists materially in giving the weight and water-resisting powers
associated with sole leather which has been largely tanned with valonia.
The valonia tannins have only a moderate affinity for hide, which, like
myrabolans, they penetrate very slowly. When used alone the leather is
less yellow than that from myrabolans, and is also duller. After most of
its bloom has been deposited valonia makes a very suitable tannage for
dressing leather, and in conjunction with gambier has been largely thus
used. Since the outbreak of war the Turkish product has, of course, not
been available for importation.

[Footnote 2: _J.S.S.I._, 1903, 1184.]

Sumach[3] is the other pyrogallol tan of commercial importance. It
consists of the leaves and small twigs of the Sicilian sumach (_Rhus
coriaria_) cultivated in Italy extensively for export. The leaves are
hand picked, dried and often ground to powder. It contains 26-28 per
cent. of a tannin which yields little or no bloom, but much gallic acid.
It is an unstable tannin, and its infusion rapidly ferments. Sumach is a
very valuable tanning material, and when used alone gives an exceedingly
durable leather of excellent light colour. It gives a soft mellow
tannage, and is therefore most suitable for light leather tanning, and
is extensively used for this purpose. It is used, nevertheless, in large
quantities by the heavy leather tanners for finishing purposes, for it
contains some organic reducing agent which exerts a powerful bleaching
action on other tannages, and which assists to brighten as well as
lighten the rather dull appearance of leathers largely tanned with
valonia. It is rather an expensive tannin, but most manufacturers find
that its results are worth its cost.

[Footnote 3: Also spelt Sumac and Shumac, and always pronounced like the
latter.]

Other pyrogallol tans are also used to a limited extent. Algarobilla and
divi-divi are the fruit pods of several species of American _cæsalpina_.
They are strong in tan (45 per cent.) and yield a light-coloured and
bright leather, but are unstable tans, yielding much bloom. Babla is a
small pod yielding a mellow tannage and much gallic acid. Celavinia is
another pod containing no colouring matter and giving an almost white
leather. The tannin is closely similar to that of oak galls. These last
were once extensively used for tanning in Austria. Willow bark is used
for tanning in Russia and Denmark. Valuable pyrogallol tannins are
obtained from oak wood and chestnut wood, but the woods are not used in
tanning as the percentage of tan is so small.

=Catechol tans=, often obtained from barks, contain usually about 60 per
cent. of carbon. They are seldom used alone, for they usually have
little or no sugar associated, and hence their liquors do not either
"sour" or "plump." They can be used alone if artificially acidified, but
without acidifying or blending would give a rather flat leather, though
possibly firm. They yield no bloom or gallic acid, but have associated
with this other characteristic substances. Of these the catechins are
the most typical, and have been considered as the parent substances of
the catechol tans.

The catechins are white crystalline substances, apparently isomers with
the general formula C{15}H{14}O{6}. They have different
melting-points, and varying amounts of water of crystallization, but are
otherwise exceedingly similar in properties. They are sparingly soluble
in cold water, but freely in hot, and in alcohol and ether. They are
precipitated by lead acetate, mercuric chloride and albumin, but not by
gelatin, tartar emetic or alkaloids. In gambier liquors they are
especially strong, and sometimes crystallize on the side of the pits,
being thus known as "whites." The phlobaphenes or "reds" are also
typical of catechol tans from which grow catechins; they can be formed
by boiling with dilute mineral acids. They are considered to be
anhydrides of the catechol tans. They are difficultly soluble in cold
water, but freely in hot, and in cold alcohol and dilute alkalies. They
are true tannins and alone are capable of making a red leather, but in
practice are often found as mud in the tan liquors owing to their
limited solubility. They naturally influence the colour of leather made
with catechol tans, which is usually distinctly redder than the leather
made from pyrogallol tans. Infusions of catechol (_cp._ catechin) give a
green-black colour with iron alum. The sodium arsenate test gives a red
colour due to catechin. The chromate and iodine tests mentioned for
pyrogallol tans give negative results with the catechol tans, but
bromine water gives a precipitate, and sulphuric acid a crimson colour.

Mimosa bark is one of the most important catechol tans. It is usually
obtained in this country from Natal ("Natal bark"); but the tree (Sydney
green wattle, _Acacia mollissima_) is a native of Australia. It is being
cultivated now extensively in South Africa, and forms a most valuable
portion of the Empire's stock of tanning material. Its more extensive
use has been long recommended by the author,[4] but its gradually
increasing employment in British tanneries has been greatly accelerated
by the war, which has prevented its delivery in Germany and has cut off
Turkish valonia from Britain. It yields about 30 per cent. of a stable
and excellent tannin, and will produce a firm, durable leather, with a
colour much less red than that obtained from many other catechol tans.
It is an astringent tan, and if carelessly used yields a harsh or even
"drawn" grain. Most of the tannin is easily extracted, yielding a clear
infusion which penetrates fairly quickly and gives good weight. It
contains less than 1 per cent. of sugar, which unfortunately rapidly
ferments to carbonic acid, so that it is not a good plumping material.
It makes in all respects an excellent blend with myrabolans. Like all
catechol tans, the resulting leather darkens on exposure to sunlight.

[Footnote 4: J.S.C.I., 1908, 1193.]

Oak bark, from _Quercus robur_, is the ancient tanning material of
Britain, and is still used to a limited extent. It contains about 13 per
cent. of tannin and is mainly a catechol tan, but also contains a
pyrogallol derivative. It yields catechin, and gives a red colour with
the sodium arsenate test, but also will yield some bloom and gallic
acid, and gives a blue-black with ferric salts. The tannin itself is
exceedingly similar to that of mimosa bark, but the material contains
about 2-1/2 per cent. of sugar, which makes it possible to employ oak
bark alone for making sole leather. It is noted for yielding a sound,
durable leather of good typical tan colour. Its tannin combines well
with hide and penetrates quickly. The fatal disadvantage of oak bark is
its weakness in tannin strength compared with other materials. This
results in heavy freight and heavy cost per unit tannin, bulky storage,
expensive handling in the factory, comparatively large bulk of spent
tan, after relatively greater trouble in extracting, and the
impossibility of making the strong liquors so necessary in these days to
produce good weight in a short time. No satisfactory extract has yet
been made from it.

Pine bark, from _Pinas abies_, is one of the staple materials of the
Continent. It contains up to 14 per cent. of a catechol tan, and, unlike
most of this group, contains a high proportion of sugar and will give
good results alone. Hemlock bark has been the staple tanning material of
North America. It is obtained from the hemlock, or _Pinus canadensis_.
It contains up to 11 per cent. of tan and much phlobaphene, and yields a
characteristic red leather of good quality, but which rapidly darkens
with sunlight. It contains some sugar, but is usually employed in
conjunction with sulphuric acid or with sugary materials. Mallet bark
yields another catechol tan similar to that of mimosa, but somewhat less
astringent and more yellow in colour. Quebracho wood and mangrove bark
have been used, but are now made into extracts.

=Leaching.=--Whatever class of leather is being made, and whatever blend
of tanning materials is being employed, the tannins must be efficiently
extracted by water in order to make the tanning liquors. This process is
called "leaching." The tanning materials, after being ground, crushed or
shredded, are placed in large pits arranged in "rounds," "sets," or
"batteries" of 6, 8 or 10 units, through which water is percolated
systematically, so as to secure a continuous extraction. Water itself is
added to only one of the pits of material. The liquor produced is passed
on to the next pit, and then to the next, and is continually gathering
strength. After passing thus through the series, the liquor becomes the
source of the strong extracted tan liquors which are used in the tannery
proper. With this system the stronger leach liquors are being acted upon
by fresh material, and the nearly "spent" material is being acted on by
the weakest liquors, and finally by water, thus ensuring a complete
extraction. In the press leach system, which is now practically
universal, the bottom of one pit communicates with the top of the next,
and the liquor presses round by gravity flow caused by a few inches
"fall." Liquor is thus constantly percolating downward through the
material in each pit. The "head leach" and "tail leach" are always
adjacent in a double row of pits, and when the material in the latter is
quite spent, it is "cast," and the pit is filled with fresh material.
The liquor is then pressed round into this pit by adding water to the
tail leach. Hot water is used to secure better diffusion. At least two
such sets of leaches ("taps" and "spenders") are necessary to spend the
material of the average tannery and to obtain liquors of the necessary
strength.

=The Manufacture of Extracts.=--In addition to the use of the natural
tanning materials described above, modern leather manufacturers employ
also a variety of "tanning extracts," _i.e._ vegetable tanning materials
in which the tannin has been already extracted, and which are supplied
in form of a solid or concentrated liquid. Such extracts only need to be
dissolved in warm water in order to make a tan liquor, and the cost and
trouble of leaching is avoided. They are a great convenience as making
strong liquors of definite strength. Many vegetable tanning materials
are too weak in tan for the tanner to leach, and indeed to justify the
cost of importation have been made available by manufacturing an extract
at the source of the material. With such weak materials the extract
manufacturer has had to secure a much more complete extraction than in
ordinary leaching, and to concentrate his infusions by means of
steam-heated vacuum pans. With such experience he has naturally begun to
make extracts also from the stronger materials, such as myrabolans and
mimosa bark, and it is now possible to have a tannery without any
leaches at all. Tanners also have begun to realize the advantages not
only of more rapid and complete extraction, but also of doing the work
for themselves, and extract factories are beginning to appear as an
adjunct to the larger tanneries. The more complete extraction of tan
also involves a greater extraction of unwanted colouring matters, hence
decolorization is a feature of extract manufacture.

=Chestnut Extract= is from the wood of the Spanish chestnut (_Castanea
vesca_), which contains 3-6 per cent. of a valuable pyrogallol tan very
similar to that of valonia. Its weight-giving and water-resisting powers
are as good as valonia, and its penetrating power is even better, so
that it forms an exceedingly suitable material for the modern short
tannage, and also for drum tannages. The extract is manufactured
extensively in France. The wood is stripped of bark and usually piled
for some months to dry and to allow the resins to become insoluble. Some
factories, however, use the green wood direct. There are two methods of
extraction, viz. in open vats and in closed vats under pressure. The two
methods yield extracts which differ in composition and properties. In
either case the vats have a capacity of up to 3,000 gallons, and hold up
to 6-1/2 tons of wood. They are arranged in series, as in leaching, and
the liquor passes in succession through all the vats over wood less and
less spent. The temperature is highest in the vat containing the fresh
water and nearly spent wood. In open vats of wood or copper the
temperature is near boiling-point, whilst in the closed autoclaves
(copper or bronze) the pressure reaches about two atmospheres and the
temperature about 130° C. (266° F.). The series may contain 5, 7, 9 or
even 12 vats, and the liquor obtained has a strength of 3° to 4-1/2°
Beaumé (22° to 33° Bkr.).

After extraction the liquor is allowed to stand, and much insoluble
matter settles out--resins, wood, fibre, etc. The clarified and settled
liquor is then passed through a cooler up to about 55° C., and then run
into the decolorizing plant, a deep vat fitted with a copper steam coil
and mechanical stirrer attached to power. The best decolorizer is
bullock's blood, which is run into the vat and well mixed. The
temperature is next raised to about 70° C., causing the blood albumin to
coagulate. It carries down with it a little tannin, but much colouring
matter. After standing a few hours the settled liquor is run off direct
to the evaporator. A multiple-effect evaporator is usually employed, and
the concentrated liquor, which has a strength of about 25° Beaumé, is
run into suitable oak casks. The extracts contain 27-32 per cent.
tannin. An extract made with open vats has about 7 per cent. soluble
non-tanning matters, whilst a "pressure extract" may contain up to 12
per cent. of these "non-tans." Pressure extracts obtain also a better
yield of tannin, which more than compensates for the slightly lower
price. Open extraction yields, however, the purer product and an extract
with better penetrating powers, and is consequently the more suitable
for drum tannages. Chestnut extract is extensively used by the heavy
leather tanners.

=Oakwood Extract= is manufactured from the wood of the common oak
(_Quercus robur_). The centre of the industry has been the oak forest of
Slavonia. The wood contains 2-4 per cent. of a tannin very similar to
that of chestnut wood, but somewhat more astringent.

The manufacture is also similar to that of chestnut extract, but
decolorization is often omitted, and greater care has to be taken and in
other ways to keep the colour within limits. One of these is to strip
the wood more completely of bark. Another is to operate at as low a
temperature as possible, about 110° C. The extraction is made in large
circular vats about 14 feet high and holding about two tons material. A
battery is composed of about eight vats or extractors. Open extraction
is used, and the liquor is passed forward after 2-3 hours' boiling, so
that the material is spent in about 24 hours. A liquor of about 5° Bé
(36 Bkr.) is obtained, and the strength of the material reduced from 4
to 1/4 per cent. of tannin. Getting rid of insoluble matter is a
difficulty, and is attained by settling, by rapidly cooling, and then
passing through a filter press of wood. For evaporation a double-effect
vacuum pan is preferred, which operates first at about 113° F., and
afterwards at 140° F. with a higher vacuum. The liquor is concentrated
from 5° to 25° Beaumé (s.g. 1.036 and 1.210 respectively).

The extract has a much higher colour than chestnut, and is not used now
as much as some years ago. As the principal supply was German, it has
been unavailable.

=Quebracho Extract= is made from the wood of the South American tree
_Loxopteryngium Lorenzii_, which contains about 20 per cent. of a
typical catechol tan. It is associated with a little catechin, much
phlobaphene, but practically no sugar. The tannin is very astringent,
penetrates quickly and gives a firm red leather which darkens on
exposure to light. It is not noted for weight-giving powers. The wood
itself, as chips or shavings, has been used in British tanneries, to a
limited extent, but the great bulk of the material is made into extract
chiefly in South America. The crude "extract," made by evaporating
aqueous infusions of the wood, is largely exported for refinement in
Europe. It is also refined on the spot to a large extent and converted
into solid extract containing 60 per cent. of tannin.

The great difficulty with quebracho has been the disposal of the
phlobaphenes, and a great variety of quebracho extracts are now
available which deal with this problem in different ways. In some the
more soluble reds are simply left in the extract under the idea that
they are really tannins and may be of some use in some part of the
tanning process; in others they have been removed by settling and
filtration at appropriate temperatures and concentrations; in most,
however, they have been solubilized by treatment with alkalies, in the
presence of reducing agents, notably by heating with sodium bisulphite
in closed vats. The base combines with the phlobaphenes, which are made
completely soluble and available for tanning. Sulphurous acid is
evolved, and its reducing powers assist materially in retaining and
promoting a good colour in the product. Such "sulphited extracts" are
now extensively manufactured in this country from the imported "crude"
extract, and sold as liquid extracts containing 30, 35 or 40 per cent.
of tan according to the requirements of the buyer; "mixed extracts"
which are solubilized quebracho blended with about 15 per cent. of
myrabolans, are also used.

By solubilizing quebracho with excess of bisulphite an extract is
obtained which possesses considerable bleaching powers, and such
extracts are also extensively manufactured for the "vatting" or
bleaching of heavy leather after tannage. The excess of sulphurous acid
not only bleaches the leather, but also swells it up and thus permits a
further absorption of strong tan liquor, which is conducive to good
weight. These bleaching extracts are usually of 36-38 per cent. strength
in tan.

=Gambier= is an extract of the leaves and twigs of the eastern shrub
_Nauclea gambir_. It is a catechol tan of peculiarly mellow quality and
great practical value. It contains much catechin, but little
phlobaphene, and yields a beautifully soft leather, but without weight.
It is an exceedingly suitable material for the early stages of tanning,
and is much liked for tanning leathers that have to be curried, and is
widely used in the manufacture of upper leather. It is, however, an
exceedingly expensive tannin, and the extract is made in a very crude
way by Chinese and Malays without much supervision. Hence its strength
in tan and general quality is extremely variable. The plant is
cultivated for the purpose of extract manufacture, and prunings are
taken in the plant's third year. They are bruised and boiled with water
in the open. The infusion is strained, concentrated, and poured into
cooling vessels in which it sets to a paste. Two varieties of gambier
are well known, "cube gambier" and "block gambier." In the latter the
extract remains as a paste containing 25 to 40 per cent. of tannin. It
is sold in oblong blocks of 1 or 2 cwt., either wrapped in cocoanut
matting or in wooden boxes. Cube gambier is made by running the
concentrated syrup into trays 2 inches deep and drying in the sun. When
partly dry, it is cut up into 1-1/2-in. cubes and dried further on
cocoanut matting. The rough "cubes" as imported contain 40-50 per cent.
of tannin.

=Myrabolans Extract= is now largely manufactured in this country. A
liquid extract of 25, 30 or even 35 per cent. strength is made for
home consumption, and a solid extract for export. The light colour,
high strength and easy extraction of the natural material have all
facilitated the task of the manufacturer.

The material is extracted in open vats or stills of copper, which take
one ton or more of nuts. A battery of 4, 6 or 8 of such stills is
usually employed, and the temperature is kept well below boiling-point
except in the vats containing the nearly spent material. The liquors
move forward quickly, and the material is quite spent in 24 hours. The
material when cast contains less than 1/2 per cent. of tannin. The
liquor obtained is 40°-50° Bkr. (6 - 7-1/2 per cent. tan), and after
settling is concentrated at 40°-50° F. in a single effect vacuum pan,
which though more costly in steam is quicker than the multiple effects,
and gives the low temperature required. For solid extract the more
concentrated liquor is run direct into tarred bags, in which it soon
solidifies.

=Hemlock Extract= is manufactured from the North American pines and
imported into this country to some extent. It gives a very red colour.

=Mangrove Extract= is made from the bark of _Rhizophona Mangle_ and
other species of mangrove which grow freely in the tropical swamps of
West Africa, Borneo, etc. Much solid and liquid extract has been made
from this material, but is not very popular on account of its harsh
tannage and dark red colour.

=Pine Bark Extract= (_Larch extract_) is made in Sweden from the Norway
spruce (_Pinus abies_). It is slightly sulphited and gives a good
colour. It is a liquid extract of about 30 per cent. strength, and is
sometimes used as a chestnut substitute. It should not be confused with
the so-called "spruce" or "pine wood" extract, which is a paper trade
bye-product and contains ligneous matters rather than tannin.

=American Chestnut Extract=, made from the chestnut oak, is either a
liquid or a solid extract in powder form. It gives a wretched
brown-black colour, which is quite unsuited to the usual British needs.

THEORY OF VEGETABLE TANNAGE.

Vegetable tannage is a phenomenon of colloid chemistry. The old
arguments as to whether tanning was a chemical or a physical process
have been rendered obsolete by the advent of a new set of explanations,
which, though shedding light on many obscure points, have enormously
increased the complexity of the problem. In vegetable tannage an
emulsoid gel (pelt) is immersed in a complex emulsoid sol (tan liquor),
which immersion results, not in simple reaction or change, but in a
series of changes.

One of these changes is _adsorption_. Pelt is a gel which possesses a
great development of surface. It not only exhibits like gelatine the
phenomenon of imbibition and dehydration to a very marked extent, but
also possesses a very fine fibrous structure due to its organic origin;
thus pelt possesses an enormous specific surface, further intensified by
the preparation processes previously discussed, which split up the hide
fibres into smaller bundles and into much finer constituent fibrils.
Tannins, on the other hand, are hydrophile colloids which in water form
emulsoid sols, and which may thus be expected to exhibit the phenomenon
of adsorption. A tan liquor usually contains several tannins in addition
to other closely similar substances, also in colloidal solution, and is
therefore a sol of considerable complexity. The immersion of pelt into a
tan liquor results in an adsorption, which consists essentially in an
inequality of concentration in the sol, the greater concentration being
at the interface. This inequality between the surface concentration and
the volume concentration of the sol, is due primarily to considerations
of surface tension and surface energy, and exists before the immersion
of the pelt. The surface layer having excess over the volume
concentration, any considerable extension of surface in a fixed volume
of sol must produce a very considerable decrease in the volume
concentration. This is what occurs when pelt is immersed in a tan
liquor, the immersion being the considerable extension of surface. It
should be especially remembered that the inequality of concentration is
in the sol, on the liquid side of the interface. In adsorption, the
substance adsorbed, _i.e._ the excess at the surface, is too frequently
regarded as bound to the solid immersed. This is because the excess is
in the layer which wets the solid and remains wetting it when the solid
is removed. Thus the immersion of pelt produces primarily only a change
in the distribution of the tannins in the liquor. It follows from this
that the adsorption is an equilibrium, and that if the sol be diluted,
the equilibrium will become the same as it would have been by immersing
the pelt directly into the dilute solution. Thus, if pelt be first
immersed in one tan liquor and then into a weaker one it will yield tan
to the latter solution.

The chief object in heavy leather tanning is to obtain the maximum
possible adsorption in the minimum possible time, or in other words, to
obtain good weight quickly. The amount adsorbed is proportional to the
actual extension of surface, _i.e._ the adsorption is a function of the
specific surface of the adsorbent. Hence, to obtain good weight it is
necessary to develop in the pelt its maximum possible specific surface.
This is one of the objects of "plumping," which splits up the fibres. It
is attained also by the solution of interfibrillar substance in limes
and bates.

The amount adsorbed is also a function of the volume concentration in
the sol after equilibrium is reached. Hence the better weights are
obtained with stronger liquors.

The adsorption law is

y/m = ac^(1/n)

where y is weight adsorbed by the weight m of adsorbent, and c the
volume concentration after adsorption; a and n are numeral constants.
Hence weight is determined by the strength of the liquor which the goods
finally leave. The commencement of tannage is necessarily in weak
infusions, in order to secure the maximum diffusion into interior of the
fibres before they become heavily coated on the exterior. As the
equilibrium is being established in such liquors the volume
concentration diminishes, and thus makes it less likely that good weight
will be attained; hence it is necessary in practice to move the goods
constantly into fresh liquors of gradually increasing strength, and so
maintain the rate of adsorption and save time. A further consequence of
the adsorption isotherm is that as y varies as c^(1/n) and n is > 1, y
is increased appreciably only by a relatively large increase in c.
Hence, though stronger liquors give better weight, there is a limit
beyond which any further gain in weight is not justified by the enormous
increase in the concentration necessary to attain it. Such great
increase in c is impracticable not only on the ground of expense, but
also on account of the great viscosity of the sol.

The amount of adsorption depends also upon the exact nature of the sol.
It has been previously pointed out that the tannins differ largely in
their penetrating and weight-giving powers. Some are readily adsorbable
and are deposited in great concentration at the surface of the fibre,
but for good weight it is necessary to use also the less adsorbable and
more diffusible tans, which penetrate the fibre itself. Hence it is
necessary for good weight to use a blend of materials, and so supply
many grades of liability to adsorption. It is particularly advantageous
to blend judiciously the two main types of material, the pyrogallol and
catechol tans. It is also necessary for good weight to present to the
pelt the more diffusible and less adsorbable tannins first, in order to
secure the maximum diffusion into the interior of the fibre before the
exterior of the fibre is heavily coated with the heavily adsorbable and
astringent tans. The least adsorbable materials are therefore used in
the early stages of tanning, and the most adsorbable materials at the
end of the tanning process. Thus gambier is added to the early liquors
(suspenders), solubilized quebracho to the later liquors (handlers), and
mimosa bark extract to the final liquors (layers). There is also another
excellent way of ensuring this progressive astringency of the liquors;
this consists in leaching the required blend of materials together (or
mixing them in the case of extracts) and presenting the mixed infusion
to the nearly tanned goods, which adsorb chiefly the more astringent
tannins. The liquor is then used for goods at a less advanced stage of
tanning, which again take the most adsorbable constituents. This is
repeated until the stage is reached when the fresh pelt is inserted into
the nearly exhausted liquor, which naturally contains only the least
adsorbable substances. This system is almost universal, and in practice
is known as "working the liquors down the yard." It has the additional
advantage of being a systematic method of economically exhausting
("spending") the tan liquors. When free acid is present in the tan
liquors, it tends to distend the fibres composing the pelt by a strong
and rapid adsorption. Thus distended or plumped the fibres present a
still greater surface for adsorptive operation, but the distension
naturally leaves less space between the fibres for the diffusion of the
sol. Hence acid or "sour" tan liquors give in the long run more weight,
but tan more slowly. Pelt tanned whilst thus plumped forms naturally a
thicker and less pliable leather. This occurs in tanning sole leather,
to a less extent with heavy dressing leather, and to a very small extent
in the case of softer dressing leathers.

In addition to adsorption, there is another phenomenon of colloid
chemistry in operation, viz. the _mutual precipitation_ of the sols in
the liquid by the gels in the hide. In most sols the disperse phase is
electrically charged. The sol therefore possesses electric conductivity,
and migration occurs in the electric field to the cathode or anode
according to the nature of the charge. Oppositely charged sols
precipitate one another, the precipitate containing both colloids. The
maximum precipitation occurs when the + charge of one sol exactly equals
and neutralizes the - charge of the other. There is thus an electrical
equivalence; an amount of sol which is equivalent to a given amount of
the other. This is not a chemical equivalence, however, and the
precipitate is not a chemical compound in spite of its fairly constant
composition. The composition of the precipitate, indeed, is not quite
constant, for the optimum precipitation may not correspond exactly with
the electrical equivalence, being influenced by the number of particles
required, their size (dispersity), the rate of mixture, and the relative
concentrations of the sols. This mutual precipitation is exhibited by
emulsoids as well as suspensoids, but the charge (+ or -) on an emulsoid
is in many instances largely an accidental matter, being determined by
the medium in which it happens to be, its normal condition being
electrical neutrality. Gelatin and pelt are such emulsoids, and a
positively charged gelatin sol has been observed to precipitate a
negatively charged gelatin sol. It is thought, however, that gelatin is
primarily a positive sol. Pelt (whether delimed or not) is rapidly
acidified by the quickly penetrating and strongly adsorbed organic acids
of the old tan liquors and becomes positively charged before the tannins
are adsorbed. The positive charge increases with the acidity of the
liquor. Other emulsoids are not electrically neutral, but are
electrically charged and exhibit considerable conductivity. Into this
class fall the tannins, and in tanning it is thought that there is a
mutual precipitation of the negative tannin sol with the positive hide
gel, the precipitation of the negative sol being favoured by the acid
condition of the liquor. The effect of increasing acidity soon falls
off, however, as a saturation limit is soon reached. This mutual
precipitation of colloids in tanning is in reality but an extension of
the adsorption theory, which explains the predominant effect of H+,
and OH- on the electric charge by stating that these ions are more
readily adsorbed than other ions, and that as OH- is more readily
adsorbed than H+ most sols are negative to water.

In addition to the adsorption phenomena described, there are in
vegetable tannage _secondary changes_ which are slow and "irreversible."
These changes are obscure and are difficult to investigate. Oxidation,
dehydration and polymerization have all been suggested, but there is
little direct evidence. Certain it is, however, that time renders the
tannage more permanent. It perhaps should be pointed out that in the
very strongest tan liquors the viscosity of the tannin sol is so great
that adhesion would be a better term than adsorption. There is no abrupt
division between the two phenomena.

In the theory of vegetable tannage there is another factor the
importance of which has been strongly emphasized by the author, viz.,
_lyotrope influence_. This has been most conveniently discussed in
connection with gelatin gels, but its effect on hide gels is analogous.
It has also an effect upon the diffusion and gelation of the tannin and
non-tannin sols.

=Mechanical Operations.=--In the tanyard the liquors are almost
invariably divided up into sections, called "rounds" or "sets," in
which the mechanical operations are different in aim and method. In
the first pits entered by the goods there is rapid adsorption in spite
of the low concentration and small astringency, and the great aim is
to obtain evenness of action and a good level colour. It is also
necessary to maintain the rate of adsorption. All the aims are
attained by frequently moving the goods. Heavy leather is suspended
vertically in the pits of tan liquor and handled up and down as well
as forward from pit to pit. Such pits are termed "suspenders." In the
earliest suspenders it is indeed advantageous to have the goods in
constant motion. This is done by suspending on wooden frames which are
rocked gently by mechanical power; such pits are termed "rockers." For
dressing leather in which firmness and smooth grain are not so
essential, the goods may be paddled in the first liquors. This is
occasionally done with stronger liquors for the express purpose of
working up the "grain" pattern. The goods after passing through the
suspenders are usually passed to "handler" rounds, in which they are
moved less frequently. In these pits the goods are laid horizontally
one above the other. One advantage of handlers is that the goods
flatten thoroughly and straighten one another by their own weight;
another is that more goods can be placed in one pit than in
suspenders. They are not so convenient to work, however, as
suspenders, and the goods do not feed so rapidly. Hence the tendency
is now to tan more in suspension, and to economize labour by an
extension of the rockers. The handling of the goods is also saved by
pumping the liquors and by working rounds of suspenders or rockers
like the press leach system, with the difference that the stronger
liquor is pumped in to the head pit, and the liquor passes upwards
through the goods.

Finally the goods are placed in "layers" or "layaways," in which they
remain undisturbed for a decidedly longer time. These pits contain the
strongest liquors of the yard, and their principal function is to
complete the tannage and give weight and firmness by the adsorption of
bloom, reds, etc., in the interior of the hide. The goods are placed in
horizontally, and are dusted in between with fresh tanning material
which maintains the local strength of the liquor and keeps the goods
somewhat apart. Drum tanning attains a more rapid penetration of the
pelt by giving constant motion in stronger infusions. It is of course
liable to result in an under-tannage of the interior of the fibre. After
the goods have been "struck through" in the ordinary way, however,
drumming in extract is increasingly used as a substitute for much labour
in handling, and also to save the time spent in the early layers.

REFERENCES.

Procter, "Principles of Leather Manufacture," pp. 220-350.

Bennett, "Manufacture of Leather," pp. 113-179.

Bennett, "Celavima and Babla," L.T.R., 1914, 122.

Dumesny and Noyer, "Manufacture of Tanning Extracts."

_Theory_:--

Meunier and Seyewetz, Collegium, 1908, 195.

Stiasny, Collegium, 1908, 117-159, 289, 294, 337.

Procter and Wilson, Collegium (London), 1917, 3.

Wilson, Collegium (London), 1917, 97, 100, 105.

Moeller, Collegium (London), 1917, 13, 38, 46, 103; and
_J.S.L.T.C._, 1917, 22, 56, 92.

Bennett, _J.S.L.T.C._, 1917, 130-133, 169-182; 1918, 40; 1920,
75-86; _S.L.R._, 1916, March.

SECTION IV.--FINISHING PROCESSES

After the tannage is complete, leather is hung up to dry. In the case of
heavy leather this drying must be very carefully carried out in order to
obtain a product of satisfactory appearance and saleable qualities.
Associated with the drying are many mechanical operations (scouring and
rolling) which assist very materially in imparting the desired
qualities. After tanning, however, the quality of the final product is
most strongly influenced by the amount of grease added in finishing.
Some grease is always used in finishing, partly because even sole
leather requires some measure of pliability and partly because a coating
of oil over the leather during drying prevents the loose tannin from
being drawn to the surface of the leather by capillarity, thereby
causing dark and uneven patches and a "cracky" grain. The added grease
is also a contribution to the "weight" of the finished article--a
primary consideration for heavy leather, which is usually sold by
weight. The finishing processes, indeed, tend to be dominated by this
consideration, and become a series of efforts to retain as much tannin
and add as much grease as are consistent with the requirements of the
class of leather being manufactured. Sole leather does not contain more
than about 2 per cent. grease, or its firmness is impaired. Belting
leather, in which considerable pliability is needed, may contain about 9
per cent., whilst harness leather, which must be exceedingly tough and
durable, may contain up to 13 per cent. of fatty matters. Upper
leathers, which need to be soft and pliable as well as waterproof and
durable, are very heavily "stuffed" and often contain up to 30-40 per
cent. of grease. Sole leather is thus rather distinct from the rest,
which are called "curried," "stuffed," or "dressed" leathers. The actual
drying out before, after and between the various mechanical operations,
each have an appropriate degree of wetness. In this country the drying
is usually under the prevailing atmospheric conditions and is known as
"weather drying." The goods are suspended by hooks or strings or by
laying over poles in special sheds fitted with louvre boards by which
the rate of drying can be roughly controlled. Weather drying is cheap,
but exceedingly slow, and in unfavourable weather is very unreliable.
The goods, moreover, need constant attention to obtain an even result.
Steam pipes are usually laid along the shed floors, and are used in
winter and damp weather to accelerate the drying, and also in the final
shed stove to remove the last traces of moisture. Wet weather, however,
will not stand a high temperature, and steam drying is better avoided
when possible. Air-dried leather still contains about 14 per cent. of
moisture. Many systems of shed ventilation have been suggested to hasten
the drying and to secure a better control of the process. In one system
a screw fan is fitted at one end of a shed (without louvre boards) and
sucks air through the goods from an inlet at the other end. The air can
be heated by a steam coil near the inlet. In another system a
centrifugal fan blows air through an arrangement of pipes which
distributes it to the drying sheds, and discharges it close to the floor
by various branch pipes. The outlets are near the roof. A system of
dampers permits hot air, warm air and the used wet air to be blended in
the desired proportions. In America turret drying has been used. The
sheds are vertically above one another and have latticed floors. Heated
air is admitted at the bottom and rises through the goods up the
building just as in a chimney. For many of the finishing operations it
is important to obtain the leather in a uniformly half dry or "sammed"
condition. This may be done by careful drying, and wetting back the
parts that have become too dry with tepid water or weak sumac liquor,
and then leaving the goods "in pile" until of uniform humidity. It may
also be done by "wetting back" leather which has been completely dried
out. There are also "samming machines" which by means of rollers squeeze
out the excess liquor. Sole leather is dried out and finished
immediately after tanning, but dressing leather is often "rough dried"
out of tan liquors and wet back for finishing when required. Dressing
leather is often treated in different factories; tanners selling it as
rough leather and "curriers" finishing it.

Scouring is one of the first operations in finishing leather. The grain
side is wet and worked with brushes and stones until the bloom and loose
tannin are removed. This process aims at producing a good even colour
and level surface, but is liable to cause a loss of weight. Dressing
leather is often scoured on both grain and flesh, and weak soap or borax
solutions are used to assist the process. In this operation hand labour
has been now quite superseded by machine work. A great variety of
machines have been devised. The mechanical working of leather takes
place in various parts of finishing. These operations, known as
"striking," "setting," "pinning," "jacking," may be carried out often by
the same machine as used for scouring, but with a change of tool. The
object of these operations is to get rid of wrinkles and creases, to
produce softness, pliability and area, and to remove superfluous
moisture, grease, dirt. The tools are of steel, brass, slate or
vulcanite. Scouring is often effected by putting the goods into rotating
drums together with extract and sumach. The bloom is removed by
friction, the colour is improved by the sumach, whilst the extract keeps
up the weight.

In finishing sole leather firmness is enhanced by "rolling." A brass
roller passes to and fro over the goods with the exertion of
considerable pressure. The operation is carried out by machinery.

Shaving is an important operation in the case of many dressing leathers.
Its object is to produce a uniform thickness of the leather and an even
surface on the flesh side. The sammed goods are laid over suitable beams
and shaved with special sharp knives which possess a turned edge. This
hand process, which demanded considerable skill, is fast becoming
extinct, and machine shaving is already almost universal on account of
its greater speed. The machines consist essentially of two rollers, one
of which is smooth, whilst the other is a spiral knife-blade cylinder
(cp. Section II.). The sammed goods are held in the hands and placed
over the smooth roller, which is raised to the cutting roller by a foot
treadle. A number of similar operations ("flatting," "whitening,"
"buffing") are carried out by a suitable change of tool. In all these
operations good samming is important.

Splitting is another important operation on tanned leather. In this
process the leather is cut parallel to its grain surface, thus yielding
two pieces with the same area as the original, the "grain" and the
"flesh split." It is essentially a machine operation, and is carried out
by presenting the carefully sammed leather to a sharp knife-edge,
towards which it must be constantly pressed. The "band knife" machine is
the most popular arrangement. The knife is an endless belt, which
continually revolves round two pulley wheels of equal size. In between
these the knife is horizontal, and is then used for splitting. The
sammed leather is pushed towards the blade by two feed rollers, and the
grain passes above the knife on to a small platform, whilst the flesh or
"split" passes below and falls to the ground. Emery grinders and thick
felt cleaners in the lower part of the machine keep the knife in good
condition. The adjustment of the machine is delicate and requires
considerable experience. With care splits may be obtained down to 1/16"
thick, and sometimes as many as 6 or 7 splits are obtained from one
hide.

Oiling is still usually done by hand, and cod oil is still preferred for
many classes of goods. Of recent years there has been a great extension
of the use of sulphonated oils, which have the valuable property of
forming an emulsion with water or tan liquor. With these materials it is
easier to ensure the goods being completely covered with oil. The
penetration of the oil into the leather is also quicker and more
complete. These oils have often the disadvantage of leaving solid fats
on the exterior of the leather, which gives it an ugly smeared
appearance.

Stuffing the dressing leathers is carried out in a variety of ways and
with a variety of materials. The old process of hand stuffing employs a
mixture of tallow and cod oil called "dubbin." This is made by melting
the ingredients together and allowing them to cool with constant
stirring to a nearly homogeneous salve. The dubbin is brushed thickly on
to the flesh side of the sammed leather, which is then hung up to dry.
As the moisture dries out the oils and soft fats penetrate the leather
and leave the more solid fats on the outside. The proportions of tallow
and oil are varied with the time of year and with the method of drying,
for if the dubbin be too soft it will run off the leather, and if too
hard will not penetrate it so well.

Drum stuffing is a more modern development in which a higher temperature
is employed, about 140° F. The drum is heated up by steam or by hot air,
and the sammed goods are then inserted and drummed for a few minutes
until they are warmed. The drum is fitted with a heated funnel
containing the melted grease, which is run in through the hollow axle.
After a half to three-quarters of an hour's drumming the grease is
completely absorbed by the leather. The drumming is continued for a
while until the goods have cooled. Whilst still warm they are "set out"
to remove creases and superfluous grease. Drum stuffing is not only
quicker than hand stuffing, but also makes it possible to use the hard
fats, and so make a leather which carries more grease without appearing
greasy. Thus in drum stuffing, paraffin wax and wool fat are used, and
their penetration assisted by small proportions of cod oil or dégras. If
the leather be too wet the grease is not absorbed, whilst if it be drier
than usual the leather will take more grease, but the resulting colour
is not so good. There is also another method of stuffing which
originates from the Continent. It is known as "burning in" and involves
the use of still higher temperatures (195° to 212° F.). Wet leather
will, of course, not stand this temperature, so that it is first
necessary to make the leather absolutely dry. This is effected by drying
in stoves at temperatures up to 110°-115° F. There are two ways in which
the grease is applied. In one method the melted grease is poured by a
ladle on to the flesh side and brushed over until evenly distributed. A
second application of grease is made to the thicker parts. The hides are
then put into warm water (120° F.) for about a quarter of an hour, and
then drummed for half an hour. In the other method the goods are
completely immersed in the melted fats for a few minutes in a
steam-jacketer tank at a temperature of 195° F. After softening in water
at 120° F. the goods are drummed. "Burning in" is used for the heavier
dressing leathers such as belting and harness. It does not give good
colour, but permits the employment of still more hard fats.

REFERENCES.

Procter, "Principles of Leather Manufacture," pp. 223, 378.

Bennett, "Manufacture of Leather," pp. 251-312.

Bennett, "Principles of Leather Stuffing," _Leather Trades Review_,
1911, 186.

SECTION V.--SOLE LEATHER

Leather

source: Project Gutenberg · page

Cite this

Hugh Garner Bennett. "Animal Proteins". Project Gutenberg. Public domain in the USA. https://www.gutenberg.org/ebooks/41192

JSON record · API collection · BibTeX · RIS · CSL-JSON · citation policy

Save to pass ·