The Project Gutenberg eBook of Leather: From the Raw Material to the Finished Product

This eBook is for the use of anyone anywhere in the United States and
most other parts of the world at no cost and with almost no restrictions
whatsoever. You may copy it, give it away or re-use it under the terms
of the Project Gutenberg License included with this eBook or online
at www.gutenberg.org. If you are not located in the United States,
you will have to check the laws of the country where you are located
before using this eBook.

Title: Leather: From the Raw Material to the Finished Product

Author: K. J. Adcock

Release date: August 1, 2013 [eBook #43377]
Most recently updated: October 23, 2024

Language: English

Other information and formats: www.gutenberg.org/ebooks/43377

Credits: Produced by Juliet Sutherland, Mary Akers and the Online
Distributed Proofreading Team at http://www.pgdp.net

*** START OF THE PROJECT GUTENBERG EBOOK LEATHER: FROM THE RAW MATERIAL TO THE FINISHED PRODUCT ***

Transcriber's note:
Spelling and punctuation inconsistencies been harmonized.
Obvious printer errors have been repaired. Italic text has been
marked with _underscores_. Bold text has been marked with
=equal signs=. Subscript numbers have been rendered, as for
example for subscript 2, as _{2}.

LEATHER

_Common Commodities and Industries Series_

Each book in crown 8vo, cloth, with many illustrations, charts, etc.
=2s. 6d.= net.

=Tea: From Grower to Consumer.= By A. Ibbetson.

=Coffee: From Grower to Consumer.= By B. B. Keable.

=Sugar: Cane and Beet.= By Geo. Martineau, C.B.

=Cotton: From the Raw Material to the Finished Product.= By R.
J. Peake.

=Rubber: Production and Utilisation of the Raw Product.= By C.
Beadle and H. P. Stevens, M.A., Ph.D., F.I.C.

=Iron and Steel: Their Production and Manufacture.= By C. Hood.

=Silk: Its Production and Manufacture.= By Luther Hooper.

=Tobacco: From Grower to Smoker.= By A. E. Tanner.

=Wool: From the Raw Material to the Finished Product.= By J. A.
Hunter.

=Coal: Its Origin, Method of Working, and Preparation for the
Market.= By Francis H. Wilson, M. Inst. M.E.

=Linen: From the Field to the Finished Product.= By Alfred S.
Moore.

=Timber: From the Forest to its Use in Commerce.= By William
Bullock.

=Clays and Clay Products.= By A. B. Searle.

=Leather: From the Raw Material to the Finished Product.= By K.
J. Adcock.

=Oils: Animal, Vegetable, Essential, and Mineral.= By C.
Ainsworth Mitchell, B.A., F.I.C.

=Wheat and its Products.= By A. Millar.

=Copper: From the Ore to the Metal.= By H. K. Picard, Assoc.
Royal School of Mines, Mem. Inst. of Min. and Met.

=Paper: Its History, Sources, and Production.= By H. A. Maddox.

=Glass and Glass Manufacture.= By Percival Marson.

=Soap: Its Composition, Manufacture, and Properties.= By
William H. Simmons.

=The Motor Industry.= By Horace Wyatt, B.A.

=The Boot and Shoe Industry.= By J. S. Harding.

=Gums and Resins.= By Ernest J. Parry.

=Furniture.= By H. E. Binstead.

_Other Volumes in preparation._

[Illustration: BLEACHING OIL-TANNED LEATHER BY EXPOSURE TO THE SUN

The Rosary Leather Mills. Ashtead]

_PITMAN'S COMMON COMMODITIES
AND INDUSTRIES_

LEATHER

FROM THE RAW MATERIAL TO THE
FINISHED PRODUCT

BY
K. J. ADCOCK

LONDON
SIR ISAAC PITMAN & SONS, LTD., 1 AMEN CORNER, E.C.4
BATH, MELBOURNE AND NEW YORK

PRINTED BY SIR ISAAC PITMAN
& SONS, LTD., LONDON, BATH,
MELBOURNE AND NEW YORK

CONTENTS

CHAP. PAGE
I. EVOLUTION OF LEATHER MANUFACTURE 1

II. HIDES AND SKINS 5

III. TANNING MATERIALS 32

IV. MACHINERY 52

V. PREPARATION OF HIDES AND SKINS FOR
TANNING 62

VI. TANNING PROCESSES 91

VII. DRESSING, DYEING, AND FINISHING OF
LEATHER 112

INDEX 159

LIST OF ILLUSTRATIONS

PAGE
BLEACHING OIL-TANNED LEATHER _Frontispiece_
MECHANICAL FLAYING 23
PIM'S SYSTEM OF FLAYING 24
WARBLE FLY 28
WARBLED KIP (584 HOLES) 29
WARBLED HIDE (MAGNIFIED) 30
TANNING EXTRACT PLANT 48
SHAVING CYLINDER 53
BLADED CYLINDER FOR BUFFING 54
BAND-KNIFE SPLITTING MACHINE 54
SHAVING KNIFE 55
SHAVING MACHINE _bet. pp._ 56 & 57
SHAVING, OLD METHOD 56
SHAVING MACHINE, KNIFE GUARD 59
SHAVING MACHINE 61
DRUM TUMBLER 67
FALLER STOCKS 67
TANNER'S BEAM 68
LIME YARD 73
DEHAIRING KNIFE 80
DEHAIRING AND FLESHING MACHINE 81
FLESHING KNIFE 83
SCUDDING KNIFE 86
BARK MILL 93
TAN-YARD 94
ROUNDING OF HIDES 95
BARKOMETER 97
PADDLE VAT 103
PINNING SOLE BUTTS 121
ROLLING MACHINE 122
ROLLING SOLE LEATHER 123
FAN FOR DRYING 124
FAN FIXED IN CHAMBER 125
SUTCLIFFE SYSTEM OF DRYING 126
SLEEKER 128
FLUFFING MACHINE 129
STRIKING-OUT AND SCOURING MACHINE 130
LEATHER-STUFFING DRUM 135
STAKING AND GLAZING MACHINE 143

LEATHER

CHAPTER I

EVOLUTION OF THE ART OF LEATHER MANUFACTURE

Before describing the making of leather by up-to-date methods, it may
be useful to attempt to outline the evolution of the ancient art of
tanning and dyeing skins. As everyone knows, leather is the preserved
skin of various animals, but the origin of the conversion of raw
skins into an imputrescible material will probably never be traced,
and it can only be assumed that the processes necessary to produce
leather from skins were gradually and, in most cases, accidentally
discovered. Long before the Christian era, the ancient Egyptians
had succeeded in bringing the manufacture of leather to remarkable
perfection, and, had they at their service the wonderful machinery
now available to the leather industry, it is certain that their
productions would have lost little or nothing by comparison with
modern leather. Happily, specimens of ancient Egyptian leather have
been preserved in one national museum, and, although they are said
to have been made at least 3,000 years ago, the colour and natural
strength of the leather are unimpaired.

Judging by the advanced state of the art of leather manufacture in
the early Egyptian period, it is obvious that the origin of its
manufacture must have considerably antedated that period, and,
indeed, it would be necessary to go back almost to the creation of
man to find the origin of the use of preserved animal skins for
clothing. The primitive method would naturally consist of simply
drying the skin, in which condition it would keep for many years
unless it came into contact with moisture, though its horniness
would no doubt cause the wearer much discomfort. It must not be
supposed that the wearing of dried raw skins with the hair left on
was impracticable, for even to-day some of the skins of fur-bearing
animals used for personal adornment are cured in this primitive
way, with the additional treatment with napthalene for disinfecting
purposes and keeping away injurious insects and moths, the object of
the limited amount of dressing being to preserve the natural strength
and coloration of the fur. In such a condition, however, the skins
are liable to acquire an unpleasant odour, and for hygienic reasons
it is advisable that all skins in the hair used for clothing or rugs
should be properly dressed, so that no decay sets in to loosen the
hair or fur.

Even now, the process of simply drying hides and skins to preserve
them before sending them to the tanner is largely practised,
especially in hot climates and in those countries where salt is not
readily available. This process of curing rests on the chemical
theory of dehydration, which, in a modified form, has recently been
successfully applied to some experiments in making leather.

Finding that the simple drying of skins would not properly prepare
them for clothing, primeval man would naturally look for some means
of treating them to conserve their original softness and pliability,
and the nearest substances at hand would be animal fats and brains.
It is almost safe to assume that this process was the first by
which hides were preserved in a state differing from their original
condition, the oxidation of the fatty matters naturally producing a
partial tannage. The effect of smoke may also have been discovered in
the earliest days of skin-curing, and it is reported that even now
one or two tribes use smoke to preserve skins.

The somewhat imperfect preservation of the hides by this method would
lead to further experiments being made, which evidently resulted in
the discovery of the tanning effect of leaves, twigs, and barks of
trees when soaked in water. It may be that the preservative effect
of alum was discovered even before the vegetable tanning process,
for the original Japanese white leather was made simply by steeping
the raw hides in certain rivers which contained a bed-rock of alum.
This primitive process is even followed to-day in one or two places
in Japan, but the leather is afterwards treated with oil to impart
tensile strength and increased suppleness. Strictly speaking, these
hides are not leather when finished, and they are quite unsuitable
for boots; but, being the toughest material known in the leather
trade, with the possible exception of raw hide, it is particularly
suitable and chiefly used for brace ends, and occasionally for
ladies' belts. It must not be inferred from reference to this process
that the Japanese only use this earliest method of making leather;
on the contrary, they are producing all classes of leather, and
especially belting and sole, by modern European methods, and it may
not be long before their competition with American and European
productions becomes an accomplished fact.

The available information seems to show that, until about thirty
years ago, the development of the industry was mainly the result
of accidental discoveries, and that the theory of tanning and
leather-dressing was imperfectly understood until within quite recent
times. Records of the leather trade 300 years ago prove that the
methods then in vogue were of the rudest kind; further, they show
that the practice of skimping the tanning process was not unknown
in those days, for a contemporaneous author describes the horny
condition of some of the leather which, despite the Government
inspection, appeared to have passed into the old Leadenhall
market for sale by the simple operation of "greasing the fist of
the seller." Spain and Hungary had by that time established the
manufacture of morocco and curried leather on a fairly sound basis,
while a few years later France began to develop the industry of
leather manufacture. Until about twenty years ago, waxed calf,
crup, calf kid, and alum-tanned kid were staple upper leathers,
together with the old Spanish cordovan leather. The sole leather
used in England was chiefly the output of tanneries in the United
Kingdom. About twenty years ago, however, the successful application
of the chrome tanning process caused quite a revolution in the
leather trade, with the result that about nine-tenths of the world's
production of boot upper leather is chrome-tanned. The introduction
of this process on a practical scale gave a great impetus to the work
of chemists, who have since made some remarkable discoveries and have
placed the art of leather manufacture on a scientific basis.

The old methods, however, are by no means obsolete, and it is
somewhat remarkable to find that a British patent was taken out last
year (1914) for converting hides and skins into leather by treating
them with brains and smoke.

CHAPTER II

HIDES AND SKINS

The hides and skins of animals form the principal raw material of
the tanner. Technically, the term "hides" is applied to the skins of
the larger animals, while the word "skins" is used in the case of
the smaller animals. Thus, the tanner speaks of ox, cow, bull and
horse _hides_, and of calf, sheep, and goat _skins_. There is an
intermediate size between a full-grown calf skin and a small hide,
and this is known as a "kip," but the line of demarcation is not very
clear.

Buyers often settle the difficulty by examining the growth marks
and the irregular substance of the skin, and, if these are marked
features, it is classified as a kip. The condition of the hides of
cattle is usually inferior during the six months after the animal
has become a yearling. East India tanned hides, which are largely
imported into England, are frequently described as E.I. "kips" in
the trade. This is hardly accurate, but the mistake is probably
due to the small size of full-grown Indian hides, which are very
little larger than the average European kips. It is interesting
to observe that furriers always refer to both their raw material
and the finished product as skins, irrespective of the size of the
fur-bearing animals. Most of the skins of wild animals are dressed
without removing the hair or fur, and this is quite a distinct trade
from leather manufacture, the only exception being the dressing
of closely cut and fine-haired calf skins for slippers and fancy
articles.

Practically every country in the world contributes to the supply of
hides and skins, but there are a few countries which are far in
advance of the others in the industries of cattle and sheep-raising.
The sources of tanners' raw material have undergone great changes
since the establishment of freezing and chilling stores for the
preparation of meat for export, and the market prices of hides are to
a large extent controlled by the supply in North and South America,
South Africa, and Australia. Whether or not the concentration of
these huge meat works into two or three centres is likely to benefit
the leather trade is a debatable point. The flaying, trimming, and
curing of hides in these establishments are certainly superior to
the work done by the average butcher, while, owing to the large
numbers of cattle slaughtered, the hides can be closely selected. On
the other hand, the value of hides and skins has risen enormously
in the last decade, the period coincident with the rapid growth
of the chilled and frozen meat industry, but the increased use
of leather in many directions may be mainly responsible for the
higher cost of the raw material, although it is obvious that the
concentration of the chief supplies of hides in a few lands must
tend to increase the severity of the competition among buyers. Apart
from the high prices of the hides, the concentration of the meat
industry in large chilling and freezing works has had the effect
of increasing the prices of beef and mutton, which are now higher
in price than freshly-killed English meat was a few years ago.
It appears to have been a grave error on the part of the British
Government when they stopped the imports of live cattle owing to the
fear of foot-and-mouth disease being communicated to domestic herds.
The disease has broken out in several places since the embargo was
imposed, so that the theory that the infection was only carried by
imported live cattle has been clearly disproved. The butchering of
cattle provides a large amount of work in subsidiary industries,
and the Government embargo on the importation of live cattle has
caused a great deal of distress in Deptford and Birkenhead, where
large abattoirs were erected for the reception of live cattle, which
used to be imported in fairly large numbers. There is no danger
of foot-and-mouth disease getting beyond the abattoirs or of the
slaughter of diseased cattle for food, and both tanners and butchers
hope to see the removal of the embargo. So far as possible, each
country should raise its own cattle to provide its own meat supply,
and this principle is recognised by many countries which prohibit the
import of foreign meat: but, owing to the rapid growth of populations
in industrial countries, with the consequent increase in the value of
land, it has become impracticable to raise enough cattle to supply
domestic needs. Even the United States of America, which formerly had
a great cattle-raising industry, has lately been obliged to import
live cattle to meet the requirements of its inhabitants. Similar
conditions prevail almost throughout Europe, and tanners have to look
to South America, Australia, and Africa for large supplies of raw
hides, although there are still some tanners in the United Kingdom
who use only the hides produced in this country.

The bulk of the production of hides and skins in the United Kingdom
is disposed of at weekly public auctions in the principal towns:
London, Manchester, Liverpool, Leeds, Birmingham, Newcastle, and
Glasgow being the largest centres of distribution. However, there
is still a large quantity bought by private treaty, and opinions
are divided as to which is the better method of buying. Before the
establishment of public auctions, hides were very cheap, but tanners
were unable to get a good selection, although, for sole leather, that
was not a very important matter. Public auctions have become so
firmly established that it would be impossible for tanners to revert
to the old system even if they desired it. The competition of private
buyers with the auction markets has certainly benefited the butcher
at the expense of the tanner, and the weighing and classification
of hides ultimately became so irregular in many markets that the
Tanners' Federation of the United Kingdom had to take strong
action not long ago to protect their interests. They demanded the
appointment of an independent inspector at each market to check the
weighing and sorting of the hides, but this was successfully resisted
by the market proprietors, who eventually agreed to the tanners
appointing travelling inspectors to visit the markets periodically.
The system is said to have improved matters.

The English markets do not collect enough hides to permit their close
sorting, so that, while the hides are graded according to weight and
quality and the sex of the animal, the question of varying substances
is generally ignored. There is usually a difference of 10 lb. in each
class where the hides are sorted by weight Ox, cow, heifer, and bull
hides are sold separately, as each sort has a different value. Bull
hides are comparatively poor in quality, owing to their irregular
substance and strong growth marks in the neck. Ox hides are the most
suitable for sole leather and belting, while cows' and heifers' are
used mainly for dressing hides, which are finished into bag, case,
strap, and boot leathers. The hides known as Scotch and Hereford
runts are the best of those produced in the United Kingdom, as they
are well-grown, compact, and well-suited to the making of sole
leather and belting. The grading of the weight of these hides at the
auction markets is generally as follows: 100 lb. and above, 90-99
lb., 80-89 lb., 70-79 lb., 60-69 lb., 59 lb. and less. This does not
give an ideal classification, as hides vary so much in texture and
substance, and it is quite possible to find spready hides of poor
substance and quality which would be heavier than a small but compact
and well-grown hide. It would be better from the tanner's point of
view if the hides were selected according to substance and quality.
There are not many bull hides grown in the United Kingdom, and in
many markets they are not classed by weight but simply into best and
secondary qualities. Horse hides are of even less value than those
of bulls, owing to their weaker texture and irregular substance.
That part of the skin under the mane is almost worthless, while the
flanks and sides are only useful for a secondary class of boot upper
leather, although some fairly good patent sides have lately been
produced from horse hide, which is suitable for that purpose owing
to its soft grain and pliable texture when tanned. The most valuable
part of a horse hide is the butt, which consists of the part known
as the "shell." This shell is covered with an extremely fine grain
which is not found in any other part of the hide. The well-known crup
leather is made from the shell of the horse hide.

In addition to hides, there are fairly large quantities of calf
and sheep skins sold at the weekly auctions, but veal is not such
an important article of food in England as it is on the Continent.
Sheep skins are far more numerous, as Great Britain is a big
mutton-consuming country. Home supplies of both hides and skins have
been greatly reduced, however, by the immense import of frozen and
chilled meat.

Although the domestic supply of hides and skins is quite inadequate
to meet the needs of British tanners, a large proportion is exported.
American tanners buy large quantities of the best hides and pickled
sheep skins. The latter are dewoolled and preserved by a process of
pickling with formic or sulphuric acid and salt before exportation.
Those preliminary operations are the work of the fellmonger. Nearly
all of the horse hides produced in the United Kingdom are, or were
before the War, sent to Germany, and British leather-dressers appear
to have lost the art of finishing horse hide, or are unable to
convert it into leather profitably.

The interchange of raw hides between various countries, and even
between those where leather manufacture is an important industry, is
somewhat remarkable, and only goes to prove that the concentration
of a particular industry in one or two centres of the world gives
these places a great advantage in regard to labour, organisation,
and technical skill, even over those countries where the raw
material is plentiful. Theoretically and economically it should
be advantageous to establish tanneries close to the supply of raw
hides, since the latter, under present conditions of preservation,
steadily deteriorate from the time they are removed from the carcase
until they reach the tannery. In some countries the methods of
preserving hides are actually so bad that the hides have often lost
half of their value before the tanner gets them. Two or three of the
largest American meat-packing establishments have erected or taken
over tanneries to deal with raw hides, one of their by-products.
Tanneries have also been erected near some of the large meat works in
the Argentine, but the development of the leather trade there is by
no means rapid, and at present the United States of America is the
largest leather-producing country in the world. Germany, France, and
the United Kingdom come next in the order named.

South Africa is an important source of supply of raw material, and
large quantities of Cape hides are sent to England. The production of
raw hides there is likely to be on a very large scale in a few years'
time, as the raising of Afrikander and other breeds of cattle is sure
to become an important industry now that the ravages of the terrible
disease, known as "tick," have been checked. China is another large
hide-exporting country; most of the hides from this source are
dried in the open air and are generally arsenicated to prevent the
ravages of insects. Immense quantities are also provided in all
other populous countries, but the demand for leather is generally
greater than the production of raw material in those countries. India
is a noteworthy exception to this general rule; the production of
Indian hides is enormous, and, although the leather trade is being
developed, there is a large surplus of raw hides and skins for
export. Large quantities are roughly tanned, however, and exported to
England, Germany, France, and other European countries to be dressed
and finished. The greater proportion of these hides and skins is used
for the making of shoe leather, while a good quantity is used for bag
(hide) and imitation morocco (goat) leathers.

Naturally, there is in the aggregate a considerable supply of raw
hides and skins from other parts of the world in addition to that
from the countries specially named, and new sources are being
frequently found.

It would be impossible to describe the characteristics of the
numerous varieties of hides and skins except in a full-sized
text-book, but a brief description of the principal sorts may be
given.

Some of the varieties produced in the United Kingdom have already
been described. In the main, there is not a great deal of difference
in the hides of various breeds, but there is a type of well-grown and
stout hides specially suitable for sole and belting leather; this
class is known as runts, and these hides are obtained from the Scotch
and Hereford breeds of cattle. The Scotch runts from the Highland
cattle are more valuable than any other class of hide found in the
United Kingdom; unfortunately, the production is small. Irish cattle
also yield good hides, but in England the interests of the cattle
owner, or feeder, are in conflict with those of the tanner, for the
system of artificially fattening cattle with oil cakes tends to make
the hides very greasy and weaker in the fibres than those hides from
animals which are reared on natural food-stuffs.

This grease is very difficult to remove and reduces the selling value
of sole leather by about 2d. per lb. The use of a borax solution for
soaking partially removes the grease, while it has been proposed that
the pelts should be treated with a solution of hyposulphite of soda
just before placing them in the tan liquors. A drawback of the latter
process is that a little weight is lost in the finished leather.

The trouble caused by the presence of a large quantity of natural
grease is even more pronounced in sheep skins than in cattle hides.
Naturally, a sheep arrives at maturity in about two years; but by the
modern system of intensive feeding with oily food-stuffs it can be
fattened in about ten months. This is obviously a great advantage to
the sheep-breeder; in other respects it is an unsatisfactory method,
for the mutton is not so well matured, and, therefore, is not so
nourishing; it contains too large a proportion of fat, and the skins
are very greasy and weak in fibre. The excess of grease does not
detract from the value of the wool, and may even be beneficial.

There are several varieties of sheep in the United Kingdom, with
widely different characteristics. A fellmonger should have a
good knowledge of the skins of various breeds in order to buy the
particular sorts that will meet the requirements of his customers,
as his business is to separate the wool from the skins and to
supply the former to the woollen factories and the latter to the
leather-dressers. He has, therefore, to study carefully both the wool
and pelt markets. While some breeds of sheep yield fine long wool of
bright lustre, others have comparatively short-stapled, and "kempy"
wool. Between these two classes, there are numerous grades, and the
task of sorting the various qualities of wool in those fellmongeries
where several classes of skins are worked is by no means easy. It is
a generally accepted axiom that the pelt (_i.e._, the skin denuded
of wool) is weaker in fibre in those skins which yield the finest
and best wool. In support of this, the Welsh mountain sheep may be
cited. This sheep has short, curly wool, but its skin is tough and
strong on the grain. In fact, it is about the only breed suitable for
roller leather, which is used in the cotton industry for covering the
drawing rollers of spinning-machines. Most of this leather is made in
North Wales, whence it is exported to every country where the cotton
industry is carried on.

Notable exceptions of the general rule regarding the relative
qualities of wool and pelts are found in two or three English
varieties, namely: the Lincolns, Leicesters and black-faced Suffolks,
which produce both fine wool and large pelts of good quality.

Other useful British breeds are the Southdowns, Devons, Shropshires,
Wensleydales, Scotch black-faced, Cotswolds, and Kerrys. Of the
imported varieties, the New Zealand and Cape sheep skins are the
best. The former, principally merino stock, not only provide very
fine wool, but also pelts of choice quality and large pattern.
Although the quality of the wool of Australian merino sheep is
little, if any, inferior to that of the New Zealand type, the skins
are not so good in quality, due, no doubt, to the hotter climate,
which is favourable to the breeding of insects and other pests which
damage the skins. The Cape sheep provide a skin which is quite
different in texture from that of any other breed. It has a certain
looseness of texture and softness of grain which make it particularly
suitable for the manufacture of glove leather.

South America is another large sheep-breeding country; but the skins
of this variety are not largely imported into England, most of them
being sent to Mazamet, the great centre of the fellmongering industry
in France. Buenos Aires skins are the most favoured of the South
American skins, owing to their large size and good substance. Monte
Videos are also very fine skins.

Smyrnas and Bagdads are other well-known varieties, but they are
generally imported in a rough-tanned condition, or, as it is known
technically, "in the crust." Leather-dressers finish them for
various purposes, but mainly for boot and shoe lining leather. When
properly tanned by the natives, these skins produce a supple finish,
especially those of the Smyrna variety. Unfortunately, many lots are
merely coloured on the surface with the tan liquor, with the result
that they dry hard and tinny; such partially-tanned leather is very
difficult to finish and is rarely satisfactory. Even when the tannage
is completed elsewhere before finishing them, they never produce such
good leather as skins properly tanned in the first instance.

Russia is another important country for the production of all kinds
of raw hides and skins suitable for leather manufacture. American
tanners buy very largely from this market, and a few enterprising
firms even send their own representatives to the great annual fair
held at Nishni Novgorod, where large quantities of dried hides and
skins, besides many other kinds of produce, are offered for sale.
British tanners take comparatively little interest in this important
supply, but, as a result of the great European War, an increase of
trade between Russia and the United Kingdom is anticipated, although
the Russian leather trade is developing rapidly and will absorb
increasing quantities of native raw material.

Excepting a few in Ireland, raw goat skins are not produced in Great
Britain. The chief drawback to goat breeding there is a somewhat
inexplicable aversion on the part of the public to the flesh of
goats; although another reason may be the destructive nature of the
animals themselves, for they devour and uproot anything edible that
comes in their way. It is, perhaps, unfortunate that some of the
large areas of uncultivated land in Great Britain are not given up
to the breeding of goats on a large scale, since these hardy animals
will thrive on rough, hilly lands. Apart from the value of the meat,
it might be a paying proposition to rear large herds of goats for
the supply of milk (which is more nourishing than cows') and skins.
Leather-dressers are, therefore, dependent on imported supplies,
of which the principal sources are India (North-Western District),
Mexico, Arabia, Africa, South America, and several European countries.

Goat skins from the main sources of supply vary very much in
quality--even those produced in the same country. In India, for
example, skins may be obtained in some districts which can be made
into leather to sell at about 5d. per square foot; from another
district, when finished into the same kind of leather, say glazed
kid, they may be worth 1s. 4d.[1] per foot. Fineness and clearness
of grain and good substance are the main essentials of a first-class
goat-skin leather; unfortunately these qualities are rarely combined
in one class of skin, and there is a decided surplus of light thin
skins which are hardly saleable, even for ladies' shoes. Some
American shoemakers overcome this difficulty by pasting a piece of
cloth on the back of the skin. In fairness to the buyer, the boots
made of such leather should be specially marked, as the wearing
quality of a backed thin leather is not to be compared with one
naturally stout.

[1] It must be understood that, owing to the war, these prices
have been greatly increased.

The skins of goats are used for many purposes besides the
manufacture of the famous glacé kid leather; gloves, moroccos for
bookbinding, upholstery for furniture, fancy articles such as purses,
pocket-books, bags, and ladies' belts all require large quantities of
goat and kid skins. It may be pointed out here, however, that quite
nine-tenths of the so-called kid gloves are made of lamb and sheep
skins. In appearance, there is very little difference between the
real kid and the lamb skin gloves, but the former are more durable
and warmer in wear than the latter.

With an enormous range of qualities, it is a difficult task for the
goat-skin dresser to find the most suitable sorts for his trade.
The skins used in the glove industry are largely obtained from
the Near Eastern countries, Arabia, Austria, Spain, and the Cape.
The selections best suited to the making of glazed and "patent"
(japanned) kid are found in the North-Western provinces of India,
Brazil, China, Russia (especially the Asiatic provinces), Mexico,
the Cape, and Arabia. The Indian goats known as the Patnas, which
are collected in the district of Behar, are commonly supposed to
be the best in the world, chiefly because of their fine grain and
stout substance; but the best Brazilian and Mexican skins are
equally good in quality. The best moroccos for fancy articles are
made from Continental skins, and in this respect Germany has the
great advantage of a good supply of native skins. Norway and Spain
also provide skins suitable for real morocco leather. A very large
quantity of Indian-tanned goat skins are imported into European
countries and dressed for "morocco" leather. There should be a
distinctive name for this class of leather, as, although it is
similar in appearance, it is not nearly so good in quality as the
real morocco.

In addition to cattle hides, sheep, and goat skins, which are the
main supply of raw material for leather, other kinds of hides and
skins are utilised. Horse hides, which, in the United Kingdom, are
graded according to size and quality in four or five selections and
sold by the piece, are largely used on the Continent, and especially
in Germany; nearly all of the British production being sold to that
country. When chrome tanned, these hides produce quite a serviceable
upper leather of good wearing quality, but, owing to their somewhat
loose texture, the characteristic grain of box calf cannot be
reproduced naturally, and the surface of the leather has, therefore,
to be printed. This style of finished leather does not meet with the
favour of British boot manufacturers, and the industry has not been
greatly developed in consequence. In view of the increasing cost of
other kinds of leather, however, more attention may be paid to that
made from horse hide, but the supply of this raw material is very
small compared to the production on the Continent, where horse flesh
is consumed freely. Russia produces large quantities of horse hides
and colt skins, most of which are exported to the United States of
America, where they are made chiefly into japanned, or so-called
"patent," leather, which commands a very high price in relation to
the cost of the raw material.

Next in importance to horse hides is the pig skin, which produces a
wonderfully tough leather. The pig skin leather industry is chiefly
confined to Scotland and Germany, the reason being that the skins are
left on the carcases in the other parts of the world. On the average,
a pig skin is worth about 6s., yet it is seldom removed from the
carcase. One reason is the great difficulty of flaying the animal; it
appears to be almost impossible by present methods to remove the skin
without cutting away a large quantity of fat, and the value of the
skin compared to the loss of weight of the meat offers very little
inducement to remove the skin, in addition to which, the custom of
leaving the rind on bacon and pork effectually prevents any attempt
at present to increase the supply of pig skins. This is a great loss
to the leather trade, for the pig skin is particularly suitable for
saddles and various kinds of strong leather goods. Imitation pig-skin
leather is made from hides, shoulders, bellies, or persians, but real
pig skin is distinguished from the imitation by its peculiarly marked
grain, formed of groups of three small holes which penetrate well
into the skin and form part of the sheaths of the pig's bristles.

Among other skins useful for leather are those of the wallaby,
kangaroo, dog, lizard, crocodile, alligator, ichneumon, frog
(Japanese), deer, antelope, and chamois, while it is said that even
rabbit skins have been pressed into service in Germany, though they
cannot have much value owing to their small size and thin substance.
Dog-skin leather wears well, mainly on account of the large amount of
natural grease present in the skin, but the supplies are naturally
small. The hides of the walrus, elephant, rhinoceros, hippopotamus,
and other wild animals are also tanned in small quantities, walrus
leather being well adapted for knife and sword polishing.

The mammals also contribute their quota to the supply of raw material
of the leather trade, the seal perhaps, being the most important.
This refers to the hairy seal hunted off the North American coast.

The raw skins are shipped chiefly from Newfoundland, where the
industry of seal fishing is well organised and provides employment
for about 6,000 men. The seal caught in the North Atlantic Ocean is
hairy and quite distinct from the fur seal captured in the Arctic
Ocean off Alaska. The skin of the hair seal is only suitable for
making into leather, but there is a layer of fat underneath it which
furnishes a valuable raw material for the manufacture of oils and
soap. The skins are salted and shipped to America and England. They
are easily distinguished from other kinds of commercial hides and
skins by the oily appearance of the flesh side.

According to an American Consular Report, the results of the fishing
during the season 1913 were satisfactory. The total number of seals
captured was 272,965, which were valued at £98,800. The number of
skins exported was 212,285, valued at £64,300, of which the United
States of America bought 151,355, the United Kingdom 60,754, and
Canada 176.

The porpoise, or sea hog, has a very useful hide which, when dressed,
makes a tough leather suitable for laces. The hides of other
cetaceous mammals, such as the whale and narwhal, are convertible
into useful leather. The British "porpoise" laces are generally made
from the skin of the white whale (_beluga_).

DEFECTS OF RAW HIDES AND SKINS

A remarkable feature of the leather trade is the great waste due
to the careless preparation of a large number of hides and skins.
Naturally, owing to their greatly increased value in recent years,
there has been a decided improvement, but much loss occurs every day
from damage to hides which ought to be avoided. The chief faults are
in flaying and curing, but there are other important defects due to
natural causes.

Bad flaying may be due (1) to cutting holes in the hides or skins;
(2) to "scoring" or "siding" (_i.e._, cutting into the hide without
going completely through), this generally occurring in the flanks or
sides which are the most difficult parts of the hide to remove from
the carcase; and (3) to mis-shaping the hide, which ought to be left
square.

Any or all of these defects may be found in a single hide. Despite
the active work of several proprietors of hide markets and the
tanners' federations the proportion of badly-flayed hides in England
constitutes a serious loss, which, however, may not fall directly on
either the butcher or the tanner, for the former may save in wages
by employing an inexperienced slaughterman, while the tanner pays a
reduced price for the hide.

The losses due to bad flaying and curing in the United Kingdom
are mainly attributable to the butchers' preference to kill these
beasts in their own back-yard rather than in a public abattoir.
Many of these small private slaughterhouses ought to be condemned
by the authorities; but very few people outside those immediately
interested have taken the trouble to inspect a modern public abattoir
where everything is provided to carry on the work expeditiously and
hygienically. On the Continent, where the conservatism of traders is
not permitted to interfere with the public welfare to such an extent
as it is in England, public abattoirs have become quite a feature in
many cities, and one of the principal results of the system has been
a remarkable improvement in the preparation of raw hides and skins
for the tanner. In fact, a mechanical method of flaying has been
invented in Paris, and is used extensively at the public abattoirs,
by which hides are removed from cattle without a single mark or
scratch. The method is known as _dépouille mécanique_ (mechanical
flaying) and consists in forcibly removing, by means of a windlass
worked by electric power, the portions of hide which adhere firmly to
the carcase and which are found over the ribs, the buttocks, and the
tail. The remaining part of the hide can be easily removed with the
ordinary butchers' flaying knife or with a heavy hammer of special
design. The apparatus required to carry out the mechanical method of
flaying, beyond the fixtures in the abattoirs where the process is
adopted, consist of two lengths of chain to hold the carcase firmly,
two special hammers, and one pair of strong pincers; the cost of one
set is about £4. Mr. Gaston Tainturier, of Paris, is the inventor of
this system, which has added thousands of pounds to the incomes of
Parisian butchers.

Figure 1 is from a photograph taken at the Islington (London)
Abattoir, where a demonstration of the process was given by Mr.
Tainturier in February, 1913.

Naturally, this method cannot be adopted in small slaughterhouses
in back-yards, but is readily adaptable to public abattoirs, where
practically all of the heavy work is done by electrical power. This
exemplifies only one of several advantages of modern abattoirs over
private slaughterhouses.

Although it cannot be expected that the English butchers will readily
change their prejudice against modern abattoirs, they are slowly but
gradually improving the flaying process in view of the high prices
paid for perfect hides. The most progressive of the proprietors of
the English hide markets are offering money prizes to slaughtermen
for the best flayed hides. Strictly speaking, this encouragement
should come from the butcher, who receives the benefit of increased
prices for hides removed without a scratch. The Tainturier system,
however, gives better results, no matter how well the hides are
removed with the knife. The method is not patented, and it is open to
anyone to adopt it merely for the cost of the apparatus, yet, despite
this gain, no butcher outside France and Belgium has yet adopted the
method, although the trade is losing hundreds of pounds every week
through bad flaying.

Several other systems of improved flaying have been devised, and
some of them patented, but very few have been adopted on a practical
scale. One of the most useful consists of fixing a safeguard about
a quarter of an inch from the edge of the knife; this prevents the
possibility of cutting holes into the hide, although it does not,
of course, prevent scoring, which is a serious defect in hides made
into sole leather. A safe method is to use a sharp knife of hard
wood, such as hickory, which has been successfully tried in one of
the large American meat-packing establishments. The hides from these
abattoirs are generally well-flayed, properly cured, and closely
trimmed, with the result that they command higher prices than any
other class of salted hides. The quotations for "packer" hides are
followed with keen interest by tanners in all parts of the world.

[Illustration: FIG. 1

MECHANICAL FLAYING

(_dépouille mécanique_)]

Another useful method of preventing damage to the hides by cuts with
a knife is that invented by Mr. E. Pim, a Liverpool hide factor.
The apparatus used is known as the tail extractor. It is of simple
construction, consisting of four pieces of iron riveted together
loosely in the shape of a diamond with a clamp attached to
secure the tail. The hide is then forcibly removed from the tail
and the buttocks by pulling it downward (Fig. 2). The importance of
this operation can be gauged from the fact that by the use of the
butcher's knife both of these parts of the hide are often cut very
badly.

[Illustration: FIG. 2

PIM'S SYSTEM OF FLAYING]

Even the apparently trivial matter of removing the hide from the
cheeks and face is economically important, for, unless those parts
are removed so as to get the maximum surface, they are only fit to
be cut off and thrown in a pit with other pieces and roundings which
are made into glue.

Imperfect preservation is another serious form of damage to hides and
one that cannot be easily remedied in some of the hot climates. Hides
and skins may be simply dried, salted and dried, wet-salted, treated
with arsenic solution and dried, brined or pickled with acid and
salt; of these methods the last-named is the most effective, but is
not practicable, or, at least, has not yet been applied practically
to the cure of hides and calf skins. Salt is not available, or is too
costly in most tropical countries; hence, Chinese, Indian, Mexican,
Colombian, and Arabian hides and skins are generally exported in
a dry condition. Even when the hides are dried under the best
conditions in a cool and shady place, they are of less value than a
fresh or a wet-salted hide, owing to a certain loss of gelatinous
matter in softening them before they can be placed in the lime
liquors. But it not infrequently happens that hides are dried by
exposure to the hot sun, or perhaps in a strong current of air. In
either case, the hide is much reduced in value and may be irreparably
ruined. The effect of submitting hides to these conditions is that
the exterior surface becomes rapidly dry and, naturally, contracted,
so that the air or heat cannot reach the interior, which retains
moisture. This moist inner layer may be quite thin, but it contains
sufficient nutrient to develop putrefactive organisms, so that when
the hide is soaked in water it practically falls to pieces. The
effect of hot sun or heat of any kind is, of course, disastrous to
raw hides and skins, and there have been not a few claims on shipping
companies as the result of storing hides near the boilers of ships.

Salt is almost invariably used for curing both hides and calf
skins, but though it is a good preservative it has one or two minor
defects. It contains too much water, and is liable to contain traces
of iron which is inimical to both raw hides and leather in process
of manufacture. Common salt is also liable to cause stains which
cannot be removed in later processes, and which are even accentuated
in the tan liquors. One trade chemist attributes these stains to
the presence of calcium sulphate (Ca. SO_{4}) or gypsum in the
salt, which is converted into calcium phosphate by the action of
the phosphoric acid in the nuclei of the hide on the sulphate of
calcium. Another well-known technical chemist is certain that stains
are produced by the growth of bacteria, and to prove his assertion
prepared in gelatine several cultures from salt-stained skins.
Practical men generally attribute the stains to the presence of
blood on the hides or skins at the time of curing, and the majority
of the stains are probably due to this cause, although the presence
of calcium sulphate as an impurity of the salt would undoubtedly
contribute to this defect. Blood contains a percentage of iron, and,
with other extraneous matters, should be washed from the hides before
salting them.

Fortunately, chemists have lately paid attention to the advantages
of the use of pure salt in various industries, with the result that
at least two chemically pure products are now available. The use of
these salts should be general for the cure of hides and skins, as
they are quite dry, and, therefore, easily spread. As a curing agent,
they are much more effective and lasting than common salt.

The use of glauber salts (Na_{2} SO_{4}) is recommended by the
International Commission for the Preservation, Cure, and Disinfection
of Hides and Skins instead of ordinary salt, where the latter is
unobtainable. The preparation of a sterilised salt, however, renders
its export a practical proposition to almost any part of the world.

Although the loss due to bad curing and flaying is very great, it is
quite small compared with the damage caused by natural defects.

The ravages of disease cause a great wastage of hides and skins, as
animals infected with anthrax are immediately destroyed and cremated
in all civilised countries, while, in Great Britain, foot-and-mouth
disease is kept in check by the same drastic method. In many other
countries, the infected cattle are isolated, treated with an
antiseptic hoof-and-mouth wash and generally cured, as it is a mild
fever which soon runs its course, although it is very contagious. The
germ of foot-and-mouth disease has not yet been discovered, for the
most powerful microscope fails to reveal its presence, but cattle
readily show the complaint, as their hoofs and mouths become covered
with swollen lesions.

Another kind of fever, known as "tick," was prevalent in the southern
part of the United States, but this disease was eventually eliminated
by systematically "dipping" the cattle three or four times a year.
The cattle "dip" used effectually prevented the ravages of the fly
which caused the disease. A similar method has of late years been
adopted in South Africa, with the result that cattle-raising in that
country is developing rapidly.

Anthrax is due to the presence of _bacillus anthracis_, a vegetable
organism of Siberian origin. Dry Chinese and Russian hides are
specially liable to contain the spores of anthrax, and, as the
disease proves fatal to workmen infected by it unless treatment with
anti-anthrax serum be given in the early stages, hides and skins
from infected areas should be disinfected before shipment. The method
proposed by Mr. A. Seymour-Jones, which consists in treating hides
with very dilute formic acid and one part of bichloride of mercury
in 1,000 of water, and afterwards with a saturated solution of salt
solution (.02 per cent.) of bichloride of mercury, seems to be the
most effective without damaging the hides.

[Illustration: WARBLE FLY

(1) Egg, (2) Larva, (3 and 4) Chrysalides, (5) Natural form of
fly, (6) Magnified fly.]

A peculiar natural defect is found in many South American goat skins,
especially the Brazilian, which are often badly scratched by the
animals rubbing themselves against cactus plants. Although, perhaps,
more of an artificial than a natural defect, the scratches caused by
cattle rubbing their hides against barbed wire constitute a serious,
but easily avoidable, loss. Such a barbarous system of fencing ought
never to be used.

[Illustration: A KIP CONTAINING 584 HOLES CAUSED BY THE WARBLE FLY

(The skin belongs to W. D. Mark & Sons, Hide Factors,
Newcastle.)]

[Illustration: FIG. 3

HOLE IN COW HIDE, MADE BY THE GRUB OF THE WARBLE FLY

(Magnified fifteen times)]

The most serious loss in connection with hides and skins, however,
is caused by the warble flies, _hypoderma bovis_ and _hypoderma
lineatum_, which lay their eggs on the hides of cattle. It has been a
debatable point for some years as to whether these eggs hatched and
burrowed their way into the hides from the exterior or were licked
and swallowed by the cattle and, after traversing the digestive
tract, pierced the hide from the interior. Professor Carpenter,
who has been experimenting a number of years for the Department
of Agriculture for Ireland, has succeeded in taking a remarkable
photograph (Fig. 3) which proves that the larvae penetrate the hide
from the exterior. These develop within the hide and often penetrate
to the flesh before they fall out to the ground and change into the
fly.

The most effective way of getting rid of the pest is to destroy the
larvae, either by cutting them out and crushing them under foot, or
by piercing them with a hot needle. No satisfactory dressing has
yet been found, but Prof. Carpenter states that sulphur dioxide is
effectual, if a good method of applying it can be devised.

While sheep skins are immune from the attacks of the warble fly, they
are often damaged by the blow-fly, lice, keds, and ticks; by scab
caused by the action of a mite or acarus; and by "cockle," which
causes a wrinkled grain. The origin of cockle is not definitely
known, but it is a seasonal defect which begins to show on a large
number of skins in December and does not disappear until the sheep
are shorn in the following spring.

CHAPTER III

TANNING MATERIALS

Tanning materials are derived from the vegetable, mineral, and animal
kingdoms.

The vegetable materials used are woods, barks, shrubs, leaves, and
fruits, either in their natural state or in the form of extracts. The
majority of the minerals have a more or less tanning effect on animal
fibres, but the principal are basic chrome salts, formaldehyde, alum
and salt. Titanium, iron, cerium and potassium salts also convert
skins into leather, but are not yet used commercially.

The animal matters that will convert skins into leather consist of
oxidised oils (chamois leather), fats, and brains (crown, Helvetia,
or Preller's leather).

Each of these classes of tanning materials has characteristic effects
which render them easily distinguishable. The use of combinations
of vegetable and mineral tannins has lately increased, and it is
possible that the blending of the two classes of materials may
produce an ideal tannage for certain classes of leather. In fact,
this result is already claimed for a chemically combined tanning
material which, according to the American patent, is prepared by the
following method: 125 lb. of solid quebracho extract is dissolved
in the same weight of hot water and allowed to cool; 16 lb. of
commercial caustic soda dissolved in two or three times its weight of
water is added, and the mixture agitated about half an hour; 150 lb.
of chromium sulphate is then added. In this way an insoluble tannate
of chrome is produced, but, on boiling and agitating, it changes
to a greenish brown colour and forms a sulphotannate of chrome. The
combination of the alum tannage and gambier (a vegetable extract)
has been used successfully for years past. Another combination which
has given good practical results is the tannage with alum and chrome
salts in the manufacture of glove leather.

The vegetable materials containing tannin should be arranged
botanically, but the following classification is simpler for
practical purposes.

NATURAL TANNING MATERIALS

1. _Barks._--Oak, Hemlock, Pine, Fir, Alder, Khaki, Willow, Cork,
Mimosa or Wattle, Babool, Larch, Mangrove, Spruce, Elm, Birch,
Pomegranate, Cebil.

2. _Leaves, Twigs, etc._--Sumach, Mangrove, Mango, Eucalyptus,
Pistacia, Lentiscus.

3. _Roots._--Canaigre, Palmetto.

4. _Fruits._--Myrobalans, Valonia, Divi-Divi, Cascalote, Mangosteen,
Pomegranate, Celavinia, Bablah, Algarobilla.

5. _Excrescences._--Gall Nuts, Chinese Galls, Pistacia Galls,
Tamarisk Galls.

TANNING EXTRACTS

1. _Woods._--Oak, Quebracho, Hemlock, Chestnut, Mimosa, Mangrove,
Spruce.

2. _Barks._--Oak, Wattle or Mimosa, Larch.

3. _Shrubs, Leaves, etc._--Gambier, Cutch, Catechu, Kino, Sumach.

4. _Fruits._--Myrobalans, Valonia.

5. _Roots._--Palmetto.

Of these materials, only about twenty are of much importance
commercially, the principal being oak, chestnut, quebracho, hemlock,
valonia, gambier, myrobalans, mimosa or wattle, sumach, mangrove,
divi-divi, spruce, larch, and babool.

OAK BARK (_quercus robur_) is still an important material, but is
rarely used alone. The bark from English oaks contains from 8-14 per
cent. of tannin (quercitannic acid) as estimated by the impregnation
of a standardised hide powder in a given quantity of the tanning
material in solution. Owing to its weakness in tannin compared with
other materials, oak bark tans very slowly. Used for sole leather,
it would not produce the essential quality of firmness and solidity,
and it is now customary to use a stronger tanning material, such as
valonia, or valonia extract, or gambier in the latter stages of the
process. This is the nearest approach to the pure oak bark tannage of
former days, and, if carefully regulated, is a great improvement on
the old method.

If dressing hides and calf skins required for boot upper leather are
bark-tanned, the tannage is often completed in a sumach liquor, the
object in this case being to lighten the colour so that the leather
can be dyed evenly.

In England, oak bark is harvested in April and May, when the sap
rises in the tree. Rings are cut round the tree soon after it is
felled and the bark is peeled from the tree with a special tool which
is forced between the bark and the wood. It is peeled in narrow
strips about 3 ft. in length, and on delivery to the tannery is
stacked in huge ricks. If harvested in a good, dry condition, the
bark is said to improve with age, although analytical tests have
shown that there is always a certain loss of tannin. An old rick is
much darker in colour than a new one, owing to exposure to the air.
Coppice bark from young trees is preferred by tanners, as it is free
from ross and generally contains more tannin than the rough bark.

In view of the modern demand for materials in extract form, English
oak bark would almost certainly be preferred in the form of a
concentrated liquid, if the supply of the raw material was plentiful
within a limited area. During the last few years it has not met with
a ready sale, owing to the large supply of other materials, but it
would doubtless regain some of its former popularity if it were
prepared in the form of an extract containing about 25 per cent.
of tannin. The only oak bark extract on the market is the American
chestnut oak (_quercus prinus_).

OAK WOOD is very largely used for the manufacture of tanning extract,
especially in Hungary and Canada. The extract contains from 24-28
per cent. of tannin, and is extensively used in the tannage of heavy
leathers, as it strengthens the liquors and hastens the process,
while keeping the quality of the leather at a high standard.

VALONIA (_quercus aegilops_) is the acorn cups of an oak tree which
grows abundantly in Asia Minor and the Greek Archipelago. No other
part but the acorn cups is exported. The harvest in Asia Minor takes
place in August, when the fruit ripens and the cups can be easily
beaten from the trees. They are left to dry on the ground and are
then sent to stores in seaport towns, and principally to Smyrna. The
drying is still further completed in spacious warehouses, where the
cups are spread out and turned over until fermentation ceases. During
this process the acorns shrink and are rejected. The cups should be
perfectly dried and very hard before export. The Turkish valonia
contains from 30 to 35 per cent. of tannin, and is of much better
quality than the Greek, which is usually harvested before it is ripe,
and, therefore, contains the acorn. As the acorn has practically no
tannin value, the Greek valonia contains only 25 to 28 per cent.
tannin. There are several grades of valonia, the best going to
Russia, Austria, and Italy. English tanners seem to prefer the lower
qualities at present, probably because the price is much less than
that of the best grade.

The beard of the valonia cup is much richer in tannin than the shell,
and, as several of the spines become detached during the storage of
the material, there is always a certain quantity of beard (_trillo_)
on offer. This may contain up to 42 per cent. of tannin, but its
price is usually the same as that of ordinary valonia. Of late years,
very large quantities of valonia have been made into extract at two
works in Smyrna. The production of extract will no doubt increase,
with a corresponding reduction in the export of the raw material.
The great advantages of the extract over the natural cup are its
superior strength of tannin (60 to 65 per cent.), easier solubility,
uniformity of quality, lower cost per unit of tan, and guaranteed
purity.

Valonia is well adapted for the tannage of sole leather in
conjunction with oak bark, for it deposits a heavy bloom (ellagic
acid), imparts weight and solidity, and increases the resistance of
the leather to moisture.

THE CHESTNUT TREE (_castanea vesca_) probably provides the next
tanning material of importance. This must not be confused with the
chestnut oak, an American tree which also yields a very useful
tannin. The chestnut is indigenous to the South of France and Italy,
where the forests have been considerably reduced in size to meet the
great demand for this popular tanning material. The greater part of
the denuded forests have not been replanted with the chestnut, as
the land has been put under cultivation whenever possible. A further
depletion has been caused by the ravages of an insect, which turns
the interior of the wood quite black and renders it unfit for
tanning purposes. It will, naturally, be several years before the
supply is exhausted, even if no reafforestation is undertaken. As
it is the most important tanning material grown in France, and the
chestnuts are used as a food, steps may be taken to cultivate the
trees on areas unsuitable for agriculture. Liquid chestnut extract
contains from 30 to 32 per cent. of tannin, and, when decolorised,
gives a light brown colour to the leather. It is rarely, if ever,
used alone, but generally in conjunction with quebracho, valonia or
myrobalan extracts.

THE CHESTNUT OAK TREE is indigenous to America and the wood yields a
very good tanning extract, containing up to 30 per cent. of tannin.
This material is the principal tanning agent used in America, where
the tannages are roughly classified in three sections: (1) oak, (2)
hemlock, and (3) the union (_i.e._, a mixture of hemlock and oak).
American tanners also use other materials to a smaller extent,
chiefly for blending with the principal tannins. Quebracho and spruce
extracts are specially favoured.

QUEBRACHO COLORADO is a tree indigenous to South America, the best
wood for tanning purposes being found in the Gran Chaco district in
the north of Argentina, and in Uruguay. The wood contains from 17 to
22 per cent. of tannin, and is so hard and heavy that it sinks in
water. In fact, its name is derived from two Portuguese words meaning
"axe-breaker."

After felling the trees, they are cut up into logs about 4 ft. in
length and either exported in this state to Hamburg, Havre, and
Liverpool, or sent to the numerous factories in close proximity to
the forests to be made into extract, in which an enormous trade has
of late years been developed. Very little of the natural material
is now used, as, even after cutting the wood into chips, the tannin
is extracted only with great difficulty, whereas the extract can be
treated with sulphites, alkalies, or neradol (the artificial tannin)
to render it easily soluble, besides which the concentration of the
material raises the percentage of its tannin to 65 or even 70 per
cent. Owing, perhaps, to faulty preparation, this tanning extract was
not well received at first, but it is now among the principal tannins
and increases in importance every year.

MYROBALANS is the unripe fruit of an Indian tree (_terminalia
chebula_) and contains from 35 to 40 per cent. of tannin which gives
a light colour to leather. This material is useful both for light
and heavy leathers, but is generally used in admixture with other
tannins. It deposits much bloom (ellagic acid) and is largely used
for brightening the dark colour produced by other tannins. A large
quantity of this material is now made into extracts, which are
more convenient to handle and more uniform in strength of tannin.
Natural myrobalans have the appearance of shrivelled nutmegs, except
that they are yellowish in colour; they are very hard and require
a special milling machine to reduce them to powder. The quality of
myrobalan nuts varies in different districts, the best being Bhimlies
and Jubbalpores.

SUMACH is a valuable tanning material, and is used for a large
proportion of the light and fancy leathers. It is a small bush plant
which grows in Italy, Spain, Southern France, America, and Algeria,
but of the numerous varieties the Sicilian (_rhus coriaria_) is by
far the most important. Sumach is one of the few materials cultivated
on an extensive scale; most tanning materials are derived from
natural sources and, chiefly owing to the length of time before trees
reach maturity, it would not be a paying proposition to cultivate
them. The sumach shrubs are propagated from small cuttings and
the leaves can be picked at the end of the first year, but it is
better to allow the shrubs to become more firmly established before
stripping them. The leaves are dried and sometimes exported whole,
especially for the use of the silk manufacturers in Lyons; but
they are more often ground to a fine powder. All sumachs should be
ventilated to remove foreign matters and all traces of iron, which
would cause dark bluish stains on the leather. "Ventilation" is
effected by passing currents of air, preferably with a fan, through a
narrow room, when the pure sumach is sent forward, while the heavier
particles of dirt and small pieces of wood remain behind. Sometimes
the process is repeated, and the best brands of sumach are generally
described as "pure, extra ventilated." As far as possible, the male
plants (_mascolino sommacco_) are cultivated in Sicily, where the
best sumach is grown. Female sumach (_femminello sommacco_), grown in
parts of Italy, is weaker in tannin than the male, but is rarely sold
separately. The serious amount of adulteration formerly practised
by the admixture of inferior plants, and particularly of lentisco
(_pistacia lentisco_) led to the Italian Government taking strong
action a few years ago, and it is now possible, for a very small sum,
to have any consignment inspected and analysed by the Government.
Lentisco is now sold separately and is used for common work.

Sumach has been successfully introduced into Australia, but its
development is retarded owing to difficulties of labour, which render
competition with the European product almost impossible. An inferior
sumach (_rhus glabra_) is grown in America, chiefly in the State of
Virginia. It contains from 15 to 20 per cent. of tannin, and produces
a darker coloured leather than Sicilian, the best qualities of which
contain 27 to 30 per cent. of tannin.

A useful test for finding out if a sumach has been adulterated is to
treat a small quantity with strong nitric acid, which destroys the
structure of the leaves. The mass is washed and neutralised with an
alkali, when the appearance of the midrib and veins of the leaves of
the common adulterants are easily recognised.

Sumach is not so much used for shoe upper leather as it formerly
was, but it is the best tanning agent for many kinds of fancy light
leathers, such as bookbinding, calf, and skivers (the grain of split
sheep skins), moroccos, furniture leather, etc. It is also less
subject to the action of the air and gaslight than any other tanning
material, and is strongly recommended for tanning purposes by a
special committee appointed by the Society of Arts to enquire into
causes of the rapid decay of leather bindings. Sumach is very useful
for brightening up the colour of leather tanned with darker tannins,
and is frequently used for improving the colour of both dressing and
sole leather. By itself, it yields an almost white leather which
affords a good foundation for the most delicate shades.

GAMBIER or TERRA JAPONICA (_uncaria gambir_) is a crude extract of
a shrub indigenous to the Malay Peninsula. Nearly the whole of the
production is shipped from Singapore. The leaves and twigs are boiled
in an iron vessel, and when the mass has become syrupy it is strained
through a rough sieve into a shallow tub, where it is cooled. The
liquor is stirred while cooling and rapidly thickens. Before it sets,
it is cut into 1 in. cubes and thoroughly dried. Good qualities
contain from 50-65 per cent. of tannin. An inferior product, called
"block gambier," is made by allowing the syrupy mass to set in large
blocks weighing about 2 cwt. each. These are packed in coarse
matting. The strength of tannin varies from 30 to 40 per cent.
Gambier is a good tanning material, but its use has been declining
for some years past owing to its being frequently adulterated with
sago and other farinaceous plants. However, a pure gambier extract,
manufactured on the latest scientific principles, has been placed on
the market, and there will undoubtedly be a revival of the use of
this valuable tannin. This pure gambier is prepared at Asahan, in
Sumatra, and is guaranteed to contain a minimum of 38 per cent. of
tannin.

Gambier can be used to advantage in keeping up the strength of bark
liquors in the tannage of sole leather and hastening the process,
while it may be used alone for the tannage of boot upper leather
and dressing hides. It produces an exceptionally mellow and plump
leather. It is preferable, however, to complete a gambier tannage
with a little oak wood or quebracho extract, in order to fix the
tannin principle of gambier, which, perhaps on account of its
viscosity, does not readily combine with the fibres of the skin.

MANGROVE or MANGLE, a tree found on the coasts of several tropical
countries, yields a useful bark for tanning purposes. At low tide,
these trees show their great arched roots standing high above the
ground. The best varieties, the _ceriops_ species, are found in the
East Indies and Bengal, and the bark of these is said to contain
sometimes nearly 40 per cent. of tannin. Other varieties contain from
15 to 25 per cent. The bark is generally made into a solid extract,
or "cutch," in which form it contains more than 60 per cent. of
tannin, It is useful to blend with other materials, such as oak wood,
chestnut, and quebracho extracts, but used by itself it imparts a
strong reddish colour to the leather. Some of the Indian varieties
are used as dyeing materials, and act as a satisfactory mordant in
dyeing leather a dark shade.

MIMOSA or WATTLE trees, which belong to the _acacia_ species,
yield bark rich in tannin. Australia is the native country of
several varieties, including the Black Wattle (_acacia pycnantha_),
the Golden Wattle (_A. longifolia_), and the Green Wattle (_A.
decurrens_).

The bark contains from 20 to 45 per cent. of tannin. The cultivation
of wattle in Australia seems to have declined, owing to the high cost
of labour and inability to compete with the mimosa bark imported from
South Africa, where it is cultivated on a very large scale and where
labour conditions are more favourable for the growers, as is clearly
shown by the fact that the wattle growers in Australia successfully
petitioned the Government a short time ago to place a duty of £1 10s.
per ton on the imported bark.

The introduction of the industry into South Africa was quite an
interesting adventure. A Mr. Vanderplank brought the seeds from
Australia to England about seventy years ago, and afterwards took
them to South Africa, where, in recognition of certain services a
few months after his arrival, he was granted a farm by the Dutch
Government. He then planted the seeds of the black wattle, which grew
so well that it was only a question of developing the industry. It
was some years before any African bark was exported, and only £11
worth was shipped in 1886. In 1911, the exports had risen to £288,000.

Wattle trees can be grown on soil that is unsuitable for agriculture,
and there is every prospect of the industry expanding in South
Africa, where a factory has lately been established for the purpose
of converting the bark into an extract, which, it is said, will
contain between 50 and 60 per cent. of tannin. By far the greater
proportion of wattle bark is still exported in the natural form,
ground or chopped, and packed into bags weighing about 1 cwt. each.
Before the European War nearly the whole of the bark was shipped to
Hamburg, English tanners taking very little interest in it, although
it was largely used by German tanners. But since the supplies of
the materials favoured by British tanners have become somewhat
restricted, attention has been drawn to the value of mimosa bark.

DIVI-DIVI (_caesalpinia coriaria_) is the dried pods of a Central
American tree. It has also been successfully cultivated in India. The
pods are rich in tannin, containing anything from 40-50 per cent.,
but its value is discounted by its liability to fermentation, which,
however, may be checked to some extent by the use of antiseptics,
such as carbolic acid, formaldehyde, or by the addition of synthetic
tannin, neradol. If this tendency to fermentation and oxidation of
the colouring matter could be checked completely, divi-divi would
be a valuable material, as it makes a firm leather of good colour.
When dried, the pods curl up in the shape of the letters S and C. The
tannin is found in the husks of the pod. The seeds, which contain
no tannin, are so hard that it has not yet been found profitable
to extract the oil from them. Very similar tanning materials to
divi-divi are cascalote, indigenous to Mexico, and algarobilla
(_caesalpinia brevifolia_) which grows in Chili. Cascalote is chiefly
used by Mexican tanners and is rarely exported. Algarobilla is not
available in large quantities, otherwise it would be largely used in
Great Britain, as it does not ferment so readily as divi-divi, and is
even richer in tannin.

CELAVINIA (also spelt celavina and cevalina) has been on the English
market since 1905, but has only lately been sold in large quantities.
The scarcity of some of the popular tanning materials since the
outbreak of the European War resulted in enquiries for materials that
were very little known, and celavinia has proved worthy of attention.
It consists of the seed pods of the tree _caesalpinia tinctoria_,
which grows abundantly in certain districts of Central and South
America. The pod is from 4 to 6 in. long and is flaky when dried. It
contains 30 to 32 per cent, of tannin of the pyrogallol class, and
gives a very light-coloured and almost white leather. It is the only
pyrogallol tannin which does not deposit bloom, or ellagic acid, on
the leather. It may be used as a substitute for sumach in tanning,
but has not the same bleaching effect in the retanning process. A
tanning extract of celavinia would be useful for some classes of
light leathers, where paleness of tint is important. It is difficult
to make a second extraction of tannin in the case of the natural
material, as, after the first extraction, it forms a soft pulp,
through which water will not easily percolate.

HEMLOCK (_abies canadiensis_) is an important tanning material, both
the bark and the wood being extensively used in America. The wood is
now generally converted into extracts in factories built near the
principal forests. Of late years, this extract has been imported into
the United Kingdom in fairly large quantities, in order to produce a
cheap red sole leather to compete with the American hemlock-tanned
leather. It contains only about 25 per cent. of tannin, but its value
is increased by its contents of insoluble non-tannins, which give
weight and solidity to the leather. Hemlock really gives a strong,
durable leather, but in America the practice of using artificial
weighing materials, such as glucose and Epsom salts, with a reduced
quantity of tanning material, has considerably lowered the value of
this leather.

In addition to the materials described, there are several of minor
importance which can only be briefly mentioned.

LARCH BARK is obtained from the tree _larix Europea_, which is found
in Scotland and North Europe. It contains 10-12 per cent. of tannin,
which gives a light colour and pleasant odour to leather. Scotch
basils (sheep skins) are tanned with this bark.

BIRCH BARK, from the white birch, _betula alba_, is another aromatic
tanning material. It contains only about 5 per cent. of tannin,
and is, therefore, generally used with other tanning materials.
It contains a tar which imparts an agreeable scent to the leather
that protects it from the ravages of insects. In conjunction with
willow bark (_salix arenaria_) it is used in the tanning process
for the real Russia leather. An oil containing the scent can be
extracted from the birch bark by dry distillation, and this extract
is sometimes used during the dyeing process, in the manufacture of
imitation Russia leather, which, however, only retains the scent for
a few months, whereas the real Russia leather has a permanent odour.

CANAIGRE (_rumex hymenosepalum_) is the tuberous root of a dock
plant indigenous to Mexico and the Southern States of America. It is
fairly rich in tannin (25-30 per cent.) and yields a moderately firm
leather. It contains too large a proportion of starch, however, and
cannot be described as a really satisfactory tannin. Moreover, it is
not harvested economically and the only way to make a satisfactory
tannin of it is to convert it into extract and remove the starchy
matters near the source of supply, if anyone dare take the risk of
establishing a factory in Mexico.

BABLAH or BABOOL (_acacia arabica_ or _acacia vera_) grows in India,
Egypt, and the Sudan. The bark of the babool tree is one of the
principal tanning materials used in India for hides, calf, and sheep
skins, which are sent in large quantities to Great Britain in a
rough-tanned state and dressed there. It contains 15-20 per cent. of
tannin, which readily oxidises in the leather in contact with light,
turning into a bright pink colour. It also seems to weaken the fibres
of animal tissues, and, for that reason, babool-tanned leather was
condemned by the Society of Arts Commission on Bookbinding.

The pods contain from 20-30 per cent. of tannin and give a mellow and
plump leather similar to that produced by gambier. The bleaching of
the material is troublesome, and it is probable that its use would be
increased if the tannin were prepared in the form of extract.

CUTCH is a crude extract made from the Indian tree _acacia catechu_.
This is the real cutch, as distinguished from the mangrove "cutch."
It is very rich in tannin (50-60 per cent.), but contains a large
proportion of insoluble matter and is, therefore, very little used
for tanning. It is well adapted for the dyeing of dark colours or
black with mineral strikers, such as chrome and iron salts; but
its chief use is for tanning fishermen's nets, which it renders
waterproof.

Commercial tannic acid, used for medicinal purposes, is prepared from
galls or excrescences on oak trees growing in Asia Minor. These galls
are caused by an insect (_cynips_) puncturing the small branches
and producing abnormal growth in the perforated parts. The acid is
gallotannic, which, if used for making leather, would produce a soft,
spongy, and nearly white leather. This tanning material is used a
little by Near Eastern tanners, but the result is unsatisfactory.

CLASSIFICATION OF TANNING MATERIALS

Tanning materials are divided into two main classes: (1) Pyrogallol,
(2) Catechol. The pyrogallol tannins give a bluish-black colour,
and the catechol tannins a greenish-black, with iron salts. Bromine
water does not precipitate pyrogallols, but causes a precipitate with
catechols. Pyrogallols yield ellagic acid (called "bloom" in the
trade), which improves the waterproof qualities of leather. On the
other hand, catechols contain a large proportion of insoluble reds,
or phlobaphenes, which are deposited between the fibres and thus give
solidity to the leather. Pyrogallol tannins give a light coloured,
soft leather, and can be used alone satisfactorily; but heavy
leathers, such as sole and belting, need a blend of both kinds of
tannin. The pyrogallol tannins include sumach, chestnut, myrobalans,
divi-divi, oakwood, algarobilla, chestnut oak, willow, and galls.
The catechols include quebracho, gambier, hemlock, mimosa or wattle,
mangrove, larch, birch, canaigre, and cutch. Oak bark and valonia
contain some of the properties of both classes of tannins.

There are sub-divisions of these two classes, arranged according to
chemical tests, by which one tanning material can be distinguished
from another.

TANNING EXTRACTS

The manufacture of extracts from vegetable tanning materials has
increased so rapidly of late years that the process of tanning has
undergone radical changes; and, whereas the tanner was limited to
three or four materials thirty years ago, he now has the choice of
about twenty good materials. These tannins can be suitably blended
to produce first-class leather. The processes in extract manufacture
are few. The wood, bark, or fruit is broken up into small pieces
and macerated in hot or cold water. The concentration of the liquid
is done in vacuum, or in an evaporator. The latest method is to
treat the tan liquor in a "triple-effect" evaporator (Fig. 4),
the object of using three compartments being to economise in steam.
This apparatus makes liquid extracts; where a powdered or crystal
extract is required, the liquid is afterwards treated in a vacuum
drying apparatus. Some extracts contain a lot of colouring matter and
insoluble substances. To overcome this defect, they are clarified
with blood albumen, sulphites, casein, or acetate of lead.

[Illustration: FIG. 4.--TRIPLE-EFFECT EVAPORATOR (Blair, Campbell
& McLean, Ltd.)]

SYNTHETIC TANNINS

The discovery of a synthetic tannin, in 1911, by Dr. Stiasny, who
was then an assistant in the Leather Industries Department of Leeds
University, created a great deal of interest in the leather trade,
and can certainly be regarded as a triumph of the application of
chemistry to industry. It was thought at first that these tannins
might play as important a part in the leather trade as the synthetic
dye-stuffs have, but it is now generally believed that this will
not be the case. Their use is likely to be as an aid to tanning,
rather than as a complete tanning agent, although it has been found
practicable to use them for one or two classes of light skins, where
it is essential that the colour of the leather should be nearly white.

The original patent was taken out in September, 1911, in Austria,
the native country of the inventor, but the patent rights have also
been protected in other countries, while the manufacture and sale of
the product passed into the hands of a large German dye firm, who
have since taken out several patents for other synthetic tannins.
The original tannin is produced by treating a sulphonated phenol
with formaldehyde. A patent had been taken out several years before
for the use of formaldehyde in tanning, but this expired early in
1911; many patents had also been granted for sulphonated phenol
preparations, chiefly as disinfectants, but it was left to Dr.
Stiasny to discover the value of combining the two chemicals by the
process of condensation. The preparation, first known as "neradol,"
is now made in England under licence, but, since the war, its cost
has been more than doubled, so that it is unlikely to replace natural
tanning materials to any great extent.

Formaldehyde itself has certain properties which are harmful to
leather, and it must be used with extreme caution and in small
quantities to avoid these defects. It is used in the leather trade
chiefly for keeping up the substance of hides during the tanning
process, and thus causing a rapid absorption of tannin. At the
beginning of the tanning process, the liquors are acidified,
preferably with a weak organic acid, which causes the fibres of
the hides to distend. It is at this stage that the formaldehyde is
used. This method, which cannot improve, but may easily damage, the
leather, is almost entirely confined to the Continent. Formaldehyde
has a hardening and tanning effect on animal tissues, and leather
treated by this process often has inferior wearing qualities.

In the case of the artificial tannin, this property of formaldehyde
is to a large extent modified by the chemical reaction with a
sulphonated phenol, the addition of which also increases its tanning
effect; but, while the tannage is very rapid, especially in the case
of light skins, leather produced solely by means of artificial tannin
has a slight tendency to dryness after being in stock for some time.

No doubt, however, methods will be found to overcome initial
difficulties, and various liquors will be prepared to meet different
requirements. The question of price remains the deciding factor as
to its use on an extensive scale, for, while it is so high, natural
tanning materials will be preferred, except in a few special cases.
According to the hide-powder method of tannin analysis, Neradol
contains about 30 per cent. of tannin, but there are many natural
tannin extracts containing nearly double the amount of tannin at
nearly half the price of the artificial tannin; the latter, however,
has a more rapid action and also produces a nearly white leather.
Another advantage of Neradol is that it prevents drawn grain, so
that, if raw hides be treated with a small quantity before tanning,
stronger vegetable tan liquors may be safely used to hasten the
process. In the manufacture of sole leather, for example, limed
hides, after washing in water, may be suspended in a solution of
Neradol containing 3 to 5 lb. per 100 gal. of water for twelve to
twenty-four hours. This quantity produces a slight tanning effect,
the hides are thoroughly delimed, and strong vegetable tan liquors
may then be used to complete the tannage without the grain of the
hide being drawn or dark in colour, as would be the case if the hides
were not first treated with the artificial tannin.

Neradol is also said to be an effective bleaching agent for tanned
leather in a 5 per cent. solution for a few hours, without any loss
of weight.

This property may also be utilised in the production of chrome
leather, where a whiter colour is required than that produced by
the ordinary chrome tannage. For this purpose it may be used in a
pickling liquor before the one-bath process, or in the second bath of
the two-bath tannage.

For dressing wool and fur skins, the synthetic tannins are much
superior to the alum and salt process.

CHAPTER IV

LEATHER WORKING MACHINERY

When it is considered that the construction of machinery for the
leather trade had barely started thirty years ago, the wonderful
variety and utility of modern machines are remarkable, and it is a
moot point whether engineering science has not played as great a part
as, or even greater than, applied chemistry.

Excepting the bark mill, various kinds of tumblers, the fulling
stocks, glazing and rolling machines, there were practically no
efficient mechanical aids to lighten the exceedingly laborious
operations incidental to leather manufacture two decades ago; but
so many improvements have lately been made in the construction of
machinery for practically every operation in the trade that most
of the machines require very little skill to work them, and can be
operated by intelligent youths after a few weeks' experience.

The change has been of great benefit to the health of the workers,
for the continual stooping over beams and sloping tables, combined
with the arduous nature of the work, was very injurious. The
reputation that tanning had as a healthy occupation was due more
to the work of the labourers than that of the skin workers. (The
old-fashioned lime-yards and tan-yards were generally in the open,
whereas modern tanneries are roofed.)

Leather trades machinery was not a success at first, probably because
it was very difficult to get the necessary information from leather
manufacturers. However, as the engineers gained more experience of
the methods of leather-making, the defects were gradually remedied
until it may be truly said that the machines now reach a high state
of perfection. It was no uncommon thing for workmen to lose a finger
or two in a machine, but such accidents are now rare, owing to
improvements in the construction of the machines.

Most of the machines used in the leather trade are of the cylinder
type, the raw skins or leather passing between two rollers, of which
the upper one performs the operation while the lower one helps to
draw the material through the machine. To prevent accidents and
control the working of machines, a third roller is often used, which
serves to "feed" the leather or skins to the working cylinders. Of
this type of safety roller, the Seymour-Jones attachment to the
shaving and buffing machine is of great importance.

[Illustration: FIG. 5

SHAVING CYLINDER]

The operations of the tannery, which are performed by cylindrical
machines, are dehairing, fleshing, scudding, samming, shaving,
scouring, striking-out, setting, boarding, buffing, graining,
printing, embossing, and blacking or colouring. The working cylinders
usually vary according to the character of the operation, although
one or two types may be used for at least three different operations.

Where cutting or paring is done, the working cylinder is fitted with
brass blades, or steel blades backed with iron. The blades are spiral
in some machines, and are so arranged that half of them converge to
the left, and half to the right (Fig. 5). When in work, this type of
cylinder not only performs the operation for which it is specially
intended, but also stretches the leather outward, by reason of the
arrangement of the blades or knives. The blades overlap one another
to obviate marking, for if the blades met exactly at the centre they
would make a line on the leather. Figure 6 shows another arrangement
of knives for the process of buffing.

[Illustration: FIG. 6

BLADED CYLINDER FOR "BUFFING" LEATHER]

[Illustration: FIG. 7

BAND-KNIFE SPLITTING MACHINE]

The most important machines outside the working cylinder type are
the splitter, and the glazer. There are several kinds of splitting
machines, but the band-knife machine (Fig. 7) is the most largely
used. This is a veritable triumph of the engineer's art, for it
is possible to make five or six layers, all about the same size,
out of one hide, although leather is only split once or twice as a
rule. Of course, sole, belting, and other thick leathers are not
usually split. The invention of the belt-knife splitting machine
revolutionised the leather trade, and there would undoubtedly have
been a great shortage of leather without it. Formerly, all the
levelling and reducing of substance was done by paring off quite
small pieces with the shaving knife (Fig. 8), a difficult and
laborious work. These parings were only suitable for pulping and
compressing into leather board; but now the flesh splits removed
by the machine can be curried, enamelled, printed, or rolled to
make serviceable leathers, although, of course, not nearly so good
in quality as the top or grain split. The main working part of the
splitting machine is an endless steel knife which passes round two
wheels placed at opposite ends of the machine. The leather is drawn
to the knife through two rollers, of which the lower one is in
sections to allow very thick parts of the hide to pass through the
machine. It would need a large volume to describe in detail all the
different machines used in the leather trade; the constructional
details of only one machine can be given, and, in view of its
importance, the shaver is selected. Reproductions of other machines
will appear in succeeding chapters.

[Illustration: FIG. 8

SHAVING KNIFE]

Nearly every leather trades' engineer constructs shaving machines,
but the Howard-Smith is described here, not because it is the most
popular (unfortunately there is a decided preference for low-priced
machines), but because it is one of the best from an engineering
point of view, and because several improvements are embodied in its
construction.

[Illustration: FIG. 9

SHAVING LEATHER

(Old method)]

This machine consists of nearly one hundred parts and each is made
of the best material available. The advantage of this is obvious when
the question of repairs is fully considered. The first Howard-Smith
machine made has been running more than four years, and has not
cost the owner a penny for repairs, beyond, of course, the expense
of replacing the blades of the working cylinders; whereas it is no
uncommon occurrence for a cheap machine to be thrown on the scrap
heap after a few years' wear. It is always advisable, therefore, to
buy machinery of the best grade.

[Illustration: FIG. 10

DRAWING OF SHAVING MACHINE]

Figure 10 represents a drawing of the shaving machine, _A_ being the
side view, and _B_ the front. The work of the draughtsman generally
appears to the uninitiated to border on the miraculous; he is often
the designer and architect of the machine, and his work is certainly
interesting and skilful.

Many of the heavy parts, such as main castings, pedestals, etc.,
are made in the foundry, which may be part of the leather trades'
engineer's works if he is in a large way of business. The finer
parts, those which might be termed the fittings, are made in the
turnery department; while the machine is assembled in the fitters'
shop.

Figure 10 _A_ shows the side, and 10 _B_ the front construction of
the shaving machine. The figures indicate, by following the arrows,
the principal parts of the machine, which are shown in detail in
sectional tracings. For example, _T._ 65, of which no working parts
are shown in the diagram of the complete machine, is reproduced in
detail in a separate drawing shown in Figure 11. Each part of the
machine is numbered and entered in a stock-book.

In describing the principal parts indicated in Figure 10, it will
give an idea of the assembling of the machine if a beginning be made
with the main iron castings. These comprise the main bed (64), two
side frames (62), and the front frame (58). The side frames are
strengthened by the ribs which form the edge, and which are about
three times as thick as the body of the casting. The object of the
front frame is to support the foot lever (59), the rocking frame (57)
carrying the rubber roll (79), and the wooden roof (75) over which
the leather is passed. The spring (76) pulls back the rocking frame
(57) when relieved by the operator removing his foot from the lever
(59). The long spring (77) lifts up the foot lever (59) when the
latter is released.

The pullies (73) are connected with the knife cylinder which shaves
the leather. The cylinder is obscured by the wheel-guard (65) and is,
therefore, shown separately. This cylinder is comprised of a shaped
piece of steel (turned out of solid metal bars of 4-3/4 in. diameter)
into which spiral steel blades are caulked with copper or brass.
When turned, the body of the cylinder is 4-5/8 in. in diameter, but
the parts forming the bearings are reduced to 1-1/2 in. The number
of blades is twelve, fourteen, or sixteen, according to the kind of
leather shaved, and to the choice of the operator.

It is interesting to note that these blades are now being made in
Sheffield, although, before the war, they had to be imported. The
knife guard (65), shown in detail in Figure 11, is an ingenious
contrivance which prevents the operator's hands being drawn into the
machine. It consists of an automatic shutter worked by a steel chain
from the foot lever. Figure 11 _a_ represents the shutter closed down
on the knife with the rubber roll, on which the leather is carried to
the knife, at a safe distance from the shutters. Fig. 11 _b_ shows
the position when the machine is shaving the leather, the guard being
clear and the rubber roll engaged with the knife.

[Illustration: FIG. 11 _a_.]

[Illustration: FIG. 11 _b_.]

In order to sharpen the blades of the cylinder, a carborundum wheel
is fixed in close proximity, its position being indicated in the
drawing by the wheel cover (67). A bracket for feeding the wheel
to the blades when grinding them is shown at 66. When grinding the
blades, the saddle (68) carries the wheel backwards and forwards
across them. A special feature of the saddle in this particular
machine is the double-thread screw, one a right hand, and the other
a left hand. The saddle (68) is actuated by a "swimmer," as the
makers term it, which engages, say, first the right-hand thread; when
the saddle has travelled to the end of its movement the "swimmer"
automatically enters the left-hand thread, and the saddle is
rotated in the opposite direction. The "swimmer" can be disengaged
instantaneously. A brush (55) is fixed near the cylinder to remove
any leather shavings adhering to the blades. It also acts to some
extent as a fan, and, by creating a current of air, carries the
leather dust away from the operator. A trough is filled with water
to catch the dust from the carborundum wheel, while the knives are
being ground. The trough should be cleared out and refilled with
clean water from time to time. It is essential that no dust from
the grinding wheel comes into contact with vegetable tanned leather
required in a natural or colour finish, otherwise it will cause iron
stains, which are difficult to remove without damaging the leather.
For this reason, the knives should not be ground while this class of
leather is being shaved.

An important detail of the machine under description is a trueing
device. Knives are often roughened owing to the carborundum wheel
wearing irregularly. The trueing device keeps the wheel perfectly
true by means of a diamond held in the end of a screw (78). Another
ingenious arrangement (patented) is a spring (79_a_) placed at the
back of the rubber roll (79), which enables the roll to spring back
when the leather, or any part of it, is too thick for the cutting
cylinder.

A unique advantage of the Howard-Smith machine is that it is
ball-bearing throughout. The main driving shaft revolves on four
massive ball-bearings in case (71). The pullies are firmly fixed
to the driving shaft with keys or feathers. Afterwards the pullies
are machined, so that the whole shaft with its pullies is perfectly
balanced, and the machine runs smoothly without vibration.

The bladed cylinder is likewise mounted on four ball-bearings.
The intermediate driving shaft (70), which is mounted on two
ball-bearings, is connected with a large drum shaft (70_a_) which, in
its turn, sets the carborundum wheel in motion.

[Illustration: FIG. 12

SHAVING-MACHINE

(Haley)]

Fig. 12 represents another make of shaving machine.

CHAPTER V

PREPARATION OF HIDES AND SKINS FOR TANNING

Before beginning a description of manufacturing processes, a precise
definition of leather may be given. Laymen usually describe leather
as "hides tanned with bark," Since the introduction of modern
processes, however, this is only partly true. In any case, the
definition is very broad.

The primary objects of treating raw hides and skins to produce
leather is to make them imputrescible and impart various degrees
of pliability. These qualities are essential, but the simpler the
methods used to attain them, the greater the strength of the leather
produced.

The number of materials that will produce leather is legion. Whereas
oak bark was almost exclusively used for tanning until the last
century, there are now at least twenty useful vegetable tanning
materials. The active ingredient of all of these materials is tannin,
a colloidal or uncrystallisable substance. Correctly speaking, the
term "tanning," used to designate the process of converting hides
into leather, should be confined to the use of vegetable tannins;
unfortunately, the trade has largely adopted the word in many other
processes of making leather. For example, large quantities of leather
are produced by the use of minerals, and especially of chrome salts;
where the latter is used, the leather is said to be "chrome-tanned,"
although "chromed" would be a more accurate definition. One mineral
process of making leather, namely, that involving the use of alum,
or alumina sulphate, and salt, is technically described as "tawing,"
The conversion of skins into leather by the use of oxidised oil is
known as "chamoising," imitation chamois leather being made by that
process. Nearly every mineral has the property of converting skins
into leather, though most of them are of little practical value.
The most successful are the chrome salts, and alum and salt. The
use of iron salts would be by far the cheapest process, if means
could be found whereby they could be successfully used. Sixty years
ago, a chemist named Knapp experimented with iron salts, but failed
to produce satisfactory leather. Patents were taken out in Austria
in the early part of 1914 for the use of iron salts in tanning,
while a patent of more recent date covers the use of iron salts
in combination with chrome salts. Neither of these appears to be
of much practical value. The cheapest and most stable iron salts,
the sulphate and chloride, have strongly acidic properties, and,
therefore, have a somewhat destructive and hardening effect on
animal fibres. The iron salt that might convert skins into leather
is the carbonate, which is difficult to prepare cheaply enough for
commercial purposes, though it is used medicinally. A basic iron salt
might also be useful, but iron tannages would only be suitable for
black leather. Oils and fats also have leather-making properties,
fish oils being used for the manufacture of "chamois" and antelope
leather. There are other methods of producing leather which are
not used on a large scale, but sufficient examples have been given
to show that an exact definition of leather cannot be summed up in
one or two words. There are now many kinds of leather produced by
varying methods, and each class requires its own definition. Broadly
speaking, however, leather is an imputrescible material produced from
the raw skins of animals, chiefly of cattle, sheep, and goats, by
treating them with tannins extracted from the barks, wood, fruit, or
leaves of trees; or with chemicals (chiefly chrome salts, or alum and
common salt); or with oils and fats.

The preliminary processes are of great importance, as they determine
to a large extent the character of the finished leather. Mistakes
made in the early processes can never be effectually remedied.

The first operation is technically known as soaking, and its object
is to cleanse the hides or skins thoroughly. This is quite simple
in the case of raw hides received direct from the slaughterhouse,
as it is merely a question of soaking them in clean, soft water for
a few hours. If the only water available is hard, 1/2 lb. of borax
should be added for every 100 lb. of raw hides. Borax is useful in
any case, as it is a splendid cleanser and a very useful chemical in
the tannery. Most of the hides used in the United Kingdom, however,
are wet-salted (_i.e._, salted in the wet state), as it has become
customary for most butchers to send hides and skins to the auction
markets in all the principal towns, where they are offered for
sale every week. It is still a debatable point among tanners as to
whether it is better to buy hides direct from the butcher or through
these markets. It is certainly a great advantage to put hides into
work quickly (although not before they are quite cool), as time is
saved in the soaking process, and there is practically no loss of
gelatinous matter. On the other hand, the tanner is able to buy just
the selection of hides that he wants from the auction markets. Under
this arrangement, several days must elapse before the tanner receives
them, and it is, therefore, absolutely necessary to preserve them,
otherwise they begin to decompose quickly. The first sign of decay is
the slipping of the hair, which, in that condition, may be pulled out
of its roots quite easily. Micro-organisms multiply rapidly in the
gelatine of the hide, the grain comes away, and decomposition sets in
so quickly that, in a few days after the removal of the hide from the
carcase, it may lose nearly half its value for tanning purposes if it
has not been preserved by salting or by drying rapidly in the shade
in a current of air. Salted hides need a more prolonged soaking than
fresh hides, as it is essential that all trace of salt be removed
before the next process, otherwise the finished leather may be flat,
and poor in quality. Usually, two days' soaking in several changes of
water is necessary. For the soaking process, fresh or salted hides
and skins are either soaked in square, cement-lined, brick pits, or
in wooden vats filled with clean, cold water. A good system is to put
a pack of skins in one huge tank filled with clean water and leave
them in soak overnight before transferring them to the ordinary pits.
Each pit will take 50 hides, or 10 dozen calf skins, or 20 dozen goat
skins. Tanners designate as a "pack" each lot of hides or skins they
work through, irrespective of the quantity.

[Illustration: FIG. 13

DRUM TUMBLER]

[Illustration: FIG. 14

FALLER STOCKS]

Besides salting them, there are other ways of curing hides and
skins, and a large proportion is simply dried or dry-salted, the
salt in the latter method being applied while the hides are moist.
Dry hides, whether "flint" (i.e., simply dried) or salted, require
special treatment to make them soft and pliable, without which it
would be impossible to convert them into leather. Soaking in plain
water is insufficient, as it would need too much time, during which
there would be a great loss of gelatine. The use of chemicals and
mechanical motion are required; sometimes chemicals alone will
thoroughly soften the hides, but this is not often the case. Both
alkalies and acids may be used for softening dried hides, and it
is difficult to say which gives the better result, although the
former are frequently used, mainly because treatment with acids is
a comparatively recent innovation. Both kinds are effective, but
the use of acids retards the loosening of the hair, although it has
been proved experimentally that acid-softened hides give a slightly
improved yield of leather compared with the effect of the alkaline
process--a noteworthy advantage where the finished leather is to
be sold by weight. The acid generally used--formic--has antiseptic
properties, and can have no harmful effect on animal tissues, as is
generally the case where mineral acids, especially sulphuric, are
used. Sulphurous acid is also said to be a good softening agent for
hides, but it is rarely used. The most satisfactory alkalies are
sulphide of sodium (crystallised or concentrated) and caustic soda,
and of these two, the sulphide is preferred in nine cases out of ten.
The quantities used vary according to the condition of the hides, but
the average is about 1 lb. of caustic soda, or 1 lb. of concentrated
sulphide of sodium (65 per cent.), or 2 lb. of crystallised sulphide
of sodium (30 per cent.) for every 100 gal. of water. Of formic
acid, 1 lb. is sufficient for 100 gal. of water. It is possible to
soften hides by these means without mechanical acid, but the time
is considerably shortened by "drumming" the hides, _i.e._, placing
them in a round or, preferably, a square tumbler fitted inside with
shelves or staves (Fig. 13). The drum is rotated mechanically for a
few hours, during which time the hides are thoroughly kneaded and
softened by the alkali. Tanners often use a machine known as the
"faller stocks" (Fig. 14), which kneads the hides very thoroughly,
though somewhat drastically. The drum method is preferable, providing
the hides can be suitably softened. An old method, and one that is
used now by some of the small firms, is to "break over" (_i.e._,
vigorously scrape) the hides with a curved blunt knife fitted into
two wooden handles. For this manual operation, the hide is placed,
flesh side up, over the tanner's beam (Fig. 15) and is then scraped
with the knife.

[Illustration: FIG. 15

TANNER'S BEAM]

Another old method, which has not yet disappeared, is to make use of
stale soak liquors, which, although efficient for softening purposes,
cause a great loss of hide substance owing to the active growth of
bacteria, which are developed as a result of the water becoming foul
and putrid with dirt, blood, and dissolved gelatinous matter. This
method of soaking is always dangerous, apart from the great loss of
gelatine, for the thin grain (hyaline layer) is liable to be eaten
away in patches, a defect which greatly reduces the value of leather.

Dried hides are not only difficult to treat successfully in the
different processes of making them into leather, but they are also
of highly speculative value, although they are well preserved when
completely dry. It sometimes happens, however, that the drying
is imperfect; it may, for example, have been so rapid that the
exterior of both sides is thoroughly dried before the air is able to
penetrate into the centre. The result is that the interior of the
hide putrefies, but there may be no indication of this until the
hides are soaked and softened, when they may fall to pieces and are
only saleable to glue makers. Again, the hides may be dried in the
hot sun and be badly blistered, with the same result as regards their
value for leather. If the hides are dried in too high a temperature,
they become horny and rarely make satisfactory leather owing to the
difficulty of softening them. It is estimated that quite 10 per
cent. of the dried hides are improperly cured and, therefore, useless
for making into satisfactory leather.

Apart from the commercial risk in buying dry hides, their import,
especially from Russia and China, is a source of danger in conveying
the disease of anthrax to workmen. It has been conclusively proved
that dried hides are much more liable than wet-salted hides to cause
infection.

So far, only one country, the United States of America, has taken
steps to prevent the importation of the disease of anthrax, although
most countries have issued regulations in regard to the precaution
to be taken to avoid infection by anthrax in those factories where
imported hides, wool, hair, and bones are treated. It would seem
that the most rational method would be to disinfect the hides before
they are shipped, as it certainly appears to be unwise to import any
form of disease; unfortunately, the first regulations issued by the
American Government proved to be impracticable, as the suggested
method had the effect of lowering the quality of the hides, and
making the preliminary operations troublesome. Their second scheme,
consisting of baling a certain number of hides in canvas disinfected
with a 0.02 per cent. solution of mercuric chloride, is more
satisfactory, for, although it may not sterilise all the anthrax
spores inside the bale, it should prevent them reaching other goods.
This Government order only applies to hides, skins, hair, and wool
coming from countries where anthrax is known to be prevalent.

The disease of anthrax is generally contracted by workers through
sores or cuts in the hand; the bacilli multiply rapidly in contact
with the blood, and the first sign of disease is usually shown by
a red swelling or pimple in the neck. If treated at this stage by
anti-anthrax serum a cure is often effected, but if treatment is
delayed the disease quickly proves fatal, the patient dying in awful
agony. The germs of the disease may also be swallowed and the disease
develop internally, but cases of this kind are rare.

Besides the danger to workers, there is the risk of cattle being
infected. The effluent from tanneries where anthrax-infected skins
are treated contains millions of bacilli, and it is doubtful if the
latter are sterilised even when the effluents are precipitated and
aërated before they are run into streams or municipal sewers. In any
case, the sediment may be infected, and this ultimately finds its way
to the land.

Until the various European Governments insist on imported hides
from anthrax-infected areas being sterilised before shipment, the
use of a disinfectant such as lysol or a similar cresylic compound,
or bichloride of mercury, seems imperative in the first process of
soaking. The use of these disinfectants would make the waste liquors
fit for discharge into sewers or streams.

The English Public Health and River Pollution Acts have had a great
effect in improving the hygiene of the tannery, although leather
manufacturers have not welcomed them, as, in some cases, they have
meant considerable expense in providing settling tanks for the
treatment of waste liquors. The Public Health Act gives power to any
town corporation to declare as offensive trades such businesses as
tanning, hide and skin merchanting, fellmongering, tallow melting,
etc., and several boroughs have taken advantage of this law. In such
cases, anyone desiring to set up business in these trades must apply
to the Town Council, who may or may not give their consent; in fact,
a few applications to establish these businesses have lately been
refused.

While the curing of wet hides with salt or in brine is more
satisfactory than drying them, the use of ordinary salt is not an
ideal method, as 10 per cent. brine dissolves hide substance. The
recent introduction of a pure dry salt (99-98 per cent.) and of a
sterilised salt for commercial purposes has to a large extent removed
the objections to ordinary salt. Dry sulphate of soda is also a
satisfactory cure. It may be that, as hygienic conditions are further
advanced in the various industries, a suitable disinfectant will have
to be used for all hides, in addition to the salt, except where the
hides are sent direct to the tannery from the slaughterhouse.

The cure of hides in hot countries, especially where cheap salt is
unavailable, is often unsatisfactory. A method of obviating this
difficulty has been found in China, where, in one or two of the
principal towns, hides and skins are preserved by freezing them in
cold-storage. Although this process stiffens the hides, it is said to
be fairly satisfactory if they are allowed to soften naturally before
soaking them. If submitted to rough treatment before the stiffness
relaxes, there is a great danger of the hide fibres being ruptured.
Freezing removes the difficulty of softening which is experienced in
treating dried hides, while it preserves the hide substance.

After the operation of soaking, hides and skins are ready to be
treated for the removal of the hair. There are several ways of
loosening the hair sheaths, but most of them consist of treating
the hides in a solution of a caustic alkali. The use of a solution
of common lime was practically universal until a few years ago, but
nowadays sulphide of sodium, red arsenic sulphide (realgar), and
caustic soda are also used, generally in admixture with the lime.
Another process consists in sweating the hides in a heated room,
preferably a damp cellar, where rapid decomposition of the hides soon
loosens the hair.

This method is rarely used in England, but a few American tanners
seem to prefer it for certain classes of hides. In the American
process, the hides are first soaked, and then cut in half down the
back, forming what are known as sides. Dry hides are subjected to
the usual mechanical operations in the faller stocks, in which they
are kneaded by two large hammers (Fig. 14), or they are drummed in
the tumbler (Fig. 13). After the sides are thoroughly softened and
drained, they are transferred to the sweat pit, which is, preferably,
a dark underground chamber. The stock requires very careful attention
as the process is risky. The temperature should never exceed 75° F.,
otherwise the hides may be irretrievably ruined. The process may take
from one to four days, according to the varying conditions of the
hides and of the weather. The loss of nitrogenous matter gives rise
to the development of a strong odour of ammonia, which is sometimes
even too pungent for the workmen. When the hair is judged to be
sufficiently loose, the sides are washed in cold water and put in
the stocks again for about ten minutes, when all the hair will be
removed; or the hair may be scraped off in the unhairing machine.
This method is not useful for sole leather, as it causes too great
a loss of gelatine, but it saves time in the production of sides
intended for boot upper leather, which is usually sold by measurement
(superficial area).

A dehairing process has lately been invented and patented, however,
which may supersede all of the methods just described. This process
consists in treating the hides with various enzymes which loosen the
hair so effectively that it can be removed more easily than the hair
of a limed hide. The fine, short hairs underneath are also removed,
whereas by the lime method a further process is needed to get rid of
these hairs. The only drawback to its use is that the inventor has
not yet been able to produce a material cheap enough to place on the
market, but as soon as this difficulty is overcome the enzyme method
may become fairly general. Neither the hair nor the gelatine of the
hide can be damaged by this method.

[Illustration: FIG. 16

LIME YARD

("Dri-ped" Tannery)]

The usual method of liming is carried out in brick pits of square
or rectangular shape with a sloping front on which the hides or
skins can be piled to drain (Fig. 16). There is a great variation in
the quality of lime, and in all cases it should be tested for the
available percentage of caustic lime. A good sample should contain
between 70 and 80 per cent. of pure lime. Buxton lime, which can be
obtained in powdered form, is particularly suitable for the ta

source: Project Gutenberg · page

Cite this

K. J. Adcock. "Leather: From the Raw Material to the Finished Product". Project Gutenberg. Public domain in the USA. https://www.gutenberg.org/ebooks/43377