The Project Gutenberg eBook of Soldering, Brazing and Welding
This eBook is for the use of anyone anywhere in the United States and
most other parts of the world at no cost and with almost no restrictions
whatsoever. You may copy it, give it away or re-use it under the terms
of the Project Gutenberg License included with this eBook or online
at www.gutenberg.org. If you are not located in the United States,
you will have to check the laws of the country where you are located
before using this eBook.
Title: Soldering, Brazing and Welding
Editor: Bernard E. Jones
Release date: May 15, 2016 [eBook #52074]
Most recently updated: October 23, 2024
Language: English
Other information and formats: www.gutenberg.org/ebooks/52074
Credits: Produced by deaurider, Harry Lamé and the Online Distributed
Proofreading Team at http://www.pgdp.net (This file was
produced from images generously made available by The
Internet Archive)
*** START OF THE PROJECT GUTENBERG EBOOK SOLDERING, BRAZING AND WELDING ***
Transcriber’s Notes:
Bold, italics, superscript and subscript text have been trancribed as
=text=, _text_, ^{text}, and _{text}, respectively. Small capitals
have been replaced with capitals. Letters between square brackets such
as [T] and [V] indicate T- and V-shaped symbols rather than letters.
More transcriber’s Notes may be found at the end of this text.
Soldering, Brazing
and Welding
EDITED BY
BERNARD E. JONES
Editor of “Work”
With 78 Illustrations
[Illustration]
FUNK & WAGNALLS COMPANY
NEW YORK and LONDON
1917
EDITOR’S PREFACE
This handbook, which explains in detail a variety of processes common to
general metalworking, has been written by a number of thoroughly
practical men, by whom it was contributed in another form to “Work,” the
illustrated weekly journal of handicrafts and mechanics. Its appeal is
to everybody who makes any attempt at working in metals, inasmuch as at
least one of the processes--soldering, brazing or welding--will be met
at a very early stage in the beginner’s experience. This handbook will
be found a complete workshop guide to the usual methods of soldering and
brazing, and will form an excellent introduction to the modern
electrical and oxy-acetylene welding processes, to do complete justice
to which, however, a separate handbook would, of course, be necessary.
If readers encounter difficulty in any of the matters treated in this
book, they have only to write to “Work,” in whose columns (but not by
post) help will be willingly afforded.
B. E. J.
CONTENTS
CHAPTER PAGE
1. VARIOUS PROCESSES OF JOINING METALS 1
2. SOFT SOLDERS 4
3. FLUXES USED IN SOFT-SOLDERING 12
4. SOFT-SOLDERING WITH THE COPPER BIT 17
5. SOFT-SOLDERING WITH BLOWPIPE OR BUNSEN BURNER 37
6. SOLDERING ALUMINIUM 57
7. WIPING JOINTS ON LEAD PIPES 64
8. HARD-SOLDERING WITH SILVER SOLDER 75
9. SOLDERING GOLD AND SILVER JEWELLERY 83
10. BRAZING 89
11. WELDING IRON AND STEEL UNDER THE HAMMER 108
12. MAKING BLOWPIPES 112
13. MANAGING BLOW-LAMPS 118
14. MAKING BLOW-LAMPS 122
15. ELECTRIC AND THERMIT WELDING BRIEFLY CONSIDERED 129
16. OXY-ACETYLENE WELDING 134
17. LEAD-BURNING 150
INDEX 155
SOLDERING, BRAZING AND WELDING
CHAPTER I
The Various Processes of Joining Metals
Apart from the use of rivets, screws, etc., metal is commonly joined by
soldering, brazing, or welding, three groups of processes that have one
thing in common--the use of heat to fuse either the metals themselves or
an alloy which is interposed to consolidate the joint. The word “solder”
is derived through the French from a Latin word meaning “solid.”
Soldering may be “soft” or “hard.” Soft-soldering uses lead-tin alloys
which are easily melted in a bunsen gas flame or with a hot iron or bit;
while hard-soldering employs a silver-copper alloy, to melt which a
mouth blowpipe at least is necessary. Brazing is hard-soldering with
spelter (brass), and a forge or a heavy blowlamp or a powerful blowpipe
must be employed to provide the heat.
Welding is a fusion process which in the past was almost entirely
confined to wrought-iron and steel, these metals possessing the property
of weldability to an extent unknown in the case of any other metals.
The blacksmith’s process of welding is to heat the iron or steel until
the surface of the metal becomes pasty, and then to bring the two pieces
into intimate contact by hammering on the anvil. Of late years the
welding of iron, steel, copper and some other metals has been rendered
possible by the use of certain electrical and chemical methods and--most
important of all--by the use of the oxy-acetylene blowpipe, the process
being known as “fusion welding” or “autogenous soldering,” the word
autogenous implying that the process is complete in itself and
independent of the use of any extraneous substance such as solder. The
thermit process, of which so much has been heard, and which is briefly
dealt with later, is the fusion welding of iron and steel by means of
the intense heat produced by the combustion of a special chemical
compound. Perhaps the oldest of the autogenous soldering processes is
“lead-burning,” in which the flame of an airo-hydrogen blowpipe is
brought to bear upon the lead, the joint being fed with a strip of the
same metal.
Soft-soldering is an operation that the beginner will not find nearly so
difficult as hard-soldering or brazing, and although the strength of
joints made by it is not nearly equal to that produced by the methods
named, it fills a useful place within its scope. It is purely a surface
union--that is, the solder adheres to the faces in contact in much the
same manner as an adhesive sticks to metal; but with the assistance of
fluxes, the contact is made so intimate that some force is necessary to
break the joint. Soft-soldering is also of use where brazing would
simply mean the ruin or destruction of the metals, as in the cases of
lead, poor-quality brass, pewter, tin, zinc, and in tinplate and
galvanised iron.
In silver-soldering and brazing, the silver or spelter that fuses to
form the joint alloys itself so intimately with the copper or brass that
it actually becomes part of the piece itself, and for all practical
purposes cannot be distinguished from it. But soft-soldering is not
always inferior to hard-soldering. Indeed, the surface nature of the
soldering often constitutes its value.
The strongest joints of all are produced by fusion welding, as will be
duly understood from later chapters.
CHAPTER II
Soft Solders
A solder should melt at a slightly lower temperature than the metals
which it unites, and should possess the quality of alloying with the two
surfaces, thus effecting a sound and true metallic joint. Ordinary soft
solders are lead-tin alloys, and the larger the proportion of lead the
commoner is the solder said to be. At an extreme is plumber’s solder,
consisting of 2 parts of lead to 1 part of tin, and, at the other, the
best blowpipe soft solder, which contains 2 parts of tin to only 1 part
of lead. In the ordinary way, a “coarse” or “common” solder is 2 parts
of lead to 1 part of tin; a “fine” or “medium” solder, 1 part of lead to
1 part of tin; and a “very fine” or “best” solder, 1 part of lead to 2
parts of tin.
=Eutectic Alloys.=--Lead-tin solders are eutectic alloys--that is, they
are examples of the phenomenon of a combination of two metals melting at
a temperature lower than one of them would if melted separately. Thus,
lead melts at about 328° C., and tin at about 232° C., yet reference to
the following table, given by Mr. A. H. Hiorns, will show that the
“commonest” solder mentioned fuses at 303° C., and the “best” at 175°
C.
_Melting points of lead-tin alloys_
_Tin %_ _Lead %_ _Melting_
_point (C.)_
10 90 303°
20 80 278°
30 70 255°
40 60 230°
50 50 205°
60 40 187°
63 37 175°
70 30 185°
80 20 198°
90 10 215°
=Hardness of Solders.=--According to the before-mentioned authority,
Saposhniko, in 1908, determined the hardness of various lead-tin alloys
by Brineli’s method, by which a steel cone is forced into the metal. The
results he obtained are as follow:
Lead 100 90 80 70 60 50 40
Tin 0 10 20 30 40 50 60
Hardness 3·9 10·1 12·16 14·5 15·8 15·0 14·6
Lead 34 33 32 30 20 10 0
Tin 66 67 68 70 80 90 100
Hardness 16·7 15·4 14·6 15·8 15·2 13·3 4·1
These results, says Mr. Hiorns, show that the hardest alloy is the one
with 66% (about 2 parts) of tin and 34% (about 1 part) of lead, which
also is the one having the lowest melting point of all the lead-tin
alloys. The results also show that tin is slightly harder than lead.
=Compositions of Soft Solders.=--As already shown, solders vary in
fusibility according to their composition, and the choice should be
determined by the nature of the work and the properties of the metal to
be soldered. Should a solder be used of too high a melting-point, the
metal will itself be fused before the solder begins to flow.
A point to be particularly observed is that the introduction of a
foreign substance into the solder--for example, the addition of a little
zinc to a pot of “very fine” solder--will utterly spoil it and render it
unworkable. To remove zinc from solder, melt the solder in a pot, take
it off the fire and stir in powdered sulphur or brimstone until the
whole is of the consistency of wet sand. Replace the pot on the fire and
melt, but do not stir the contents. The sulphur and zinc will rise to
the surface and form into a cake. Now take the pot off the fire and
carefully remove the cake without breaking by employing two pieces of
hoop iron with bent ends.
It is false economy to use a rough solder for fine work on the score of
cheapness, since more solder is required for a given job on account of
the rough particles of solder clinging to the work; moreover, the rough
appearance of the soldering may completely spoil the job.
The table on the opposite page gives the fluxes and the compositions of
soft solders suited to a number of different metals.
=Making Solder Strips, Wire, Tears, etc.=--Only clean, pure tin and pure
lead should be employed. The lead is first melted and then the tin
added. When all is melted, place a piece of resin on the molten metal
to act as a flux, and after well stirring, the solder is made into
strips by pouring from a ladle. Solder should not be poured into sand.
It may be poured into strips on an oiled sheet of black iron, preferably
corrugated to accommodate the strips. In the absence of a corrugated
iron sheet, some workers use a ladle resembling a large spoon with a
hole about 1/16 in. in diameter near the end. To form the strips, get a
ladle full of solder, place it on a flat iron sheet; then, tilting the
ladle to allow the solder to flow over the hole, quickly draw the ladle
across the sheet. A thin strip of solder should thus be formed, and the
thickness of the strip may be varied by increasing or decreasing the
diameter of the hole in the ladle. A button of solder usually forms at
one or both ends of the strip, and this excess should be melted off the
strips by just dipping the ends into the molten solder in the pot.
SOFT SOLDERS FOR VARIOUS METALS
----------------+--------------------------+--------------------------
| | _Soft Solder_
| +------+------+------------
_Metal to be | _Flux_ | | | _Other
soldered_ | |_Tin_ |_Lead_| constit-
| | | | uents_
----------------+--------------------------+------+------+------------
Aluminium | stearin | _see table on p. 59_
Brass { |[1]zinc chloride, resin { | 66 | 34 |
Gunmetal { | or ammonium { | 63 | 37 |
Copper { | chloride { | 60 | 40 |
Lead | tallow or resin | 33 | 67 |
Block tin | zinc chloride | 99 | 1 |
Tinplate | zinc chloride or resin | 64 | 36 |
Galvanised steel| hydrochloric acid | 58 | 42 |
Zinc | hydrochloric acid | 55 | 45 |
Pewter | gallipoli oil | 25 | 25 | bismuth, 50
Iron and steel | ammonium chloride | 50 | 50 |
Britannia metal | tallow or resin | 25 | 25 | bismuth, 50
Gold | zinc chloride | 67 | 33 |
Silver | zinc chloride | 67 | 33 |
Bismuth | zinc chloride | 33 | 33 | bismuth, 34
----------------+--------------------------+------+------+------------
[Footnote 1: Zinc chloride is the ordinary “killed spirits.”]
Solder wire is very handy for small work, and can be made in the
following way: Roll a sheet of stiff writing or drawing paper into a
conical form, rather broad in comparison with its length; make a ring of
stiff wire to hold it in, attaching a suitable handle to the ring. The
point of the cone should first of all be cut off to leave an orifice of
the size required. It should then be filled with molten solder, and held
above a pail of cold water, and the stream of solder flowing from the
cone will solidify as it runs and form the wire. If held a little
higher, so that the stream of solder breaks into drops before striking
the water, it will form handy elongated “tears” of metal; when it is
held still higher, each drop forms a thin concave cup or shell, and each
of these forms will be found to have its own peculiar uses in blowpipe
work.
The method adopted for granulating tinman’s solder, which is very rarely
called for, is as follows: Place a piece of wood, well greased, over a
tub containing water, and by gently pouring the molten alloy from a
distance in a small stream on to the greased board, the metal is broken
up into a large number of very fine shots, which run off the board into
the water and are immediately cooled. The fine shots are then taken
from the water and gently dried.
=Making Solder from Pewter.=--This alloy is composed of variable
proportions of tin and lead, the average composition being about 4 parts
of lead to 1 part of tin. If old pewter is to be utilised for making
solder, tin will have to be added to the molten pewter. Thus, to convert
5 lb. of average pewter to “coarse” or “common” solder, add 1 lb. of
tin; to “fine” or “medium,” add 3 lb. of tin; and to “very fine” or
“best,” add 7 lb. of tin. The respective proportions of lead and tin
will then be 2 and 1; 1 and 1; and 1 and 2. After the proper quantity of
tin has been added, mix some powdered sal-ammoniac with the molten
metals, and well stir the alloy; it is then ready for pouring into the
moulds.
=Making Coarse Solder from Composition Piping.=--Good composition piping
is made of nearly all tin, or an alloy of tin and lead, in which the
former metal is in excess, and formerly was much used by plumbers in the
making of coarse solder, as the material consisted of odd pieces of
small value. As, however, a great deal of composition tubing is made out
of old metals of which lead, tin, antimony, arsenic, and zinc form the
alloy, it is not advisable to introduce it into solder. Should it be
done, the melting point of the solder would be raised, and in applying
it to the lead to be joined together, would probably partly melt it.
Neither do the metals named alloy in a thorough manner, but partake more
of the nature of a mixture in which the constituents partly separate
when making the joints, and some, especially zinc, show as small bright
lumps on the surface. Joints wiped with what is usually called “poisoned
metal” are difficult to make, almost invariably leak when on water
service pipes, and are dirty grey, instead of bright and clean. The zinc
could be removed from the mixture by the method already given.
=Combined Solder and Flux.=--This consisted of equal parts of lead and
tin made into fine tubing and afterwards filled with flux having resin
as a base. “Tinol” is a paste made of finely powdered solder and a
special flux, and there is also “Tinol wire” having a core of flux.
A “magic” solder, sold by hawkers, consists of the above tubular
flux-filled solder of such low melting point that it can be fused in the
flame of a lighted match.
=Soft Solders that Melt in Boiling Water.=--The following soft solders
melt at a temperature lower than that of boiling water: 1 part tin, 1
part lead, and 2 parts bismuth, melting point about 200° F.; 8 parts
lead, 4 parts tin, 15 parts bismuth, and 3 parts cadmium, melting point
140° to 150° F.; 6 parts lead, 7 parts bismuth, and 1 part cadmium,
melting point about 180° F. To ensure the alloys melting at the
temperatures stated, the metals of which they are formed should be free
from impurities, and care should be taken to prevent oxidation while
making the alloys. When melting the metals, that having the highest
melting point should be melted first, with a layer of resin over it, the
other metals being added in the order of their melting points. The alloy
should then be well stirred with a wooden stick, and poured quickly into
moulds.
=Re-melting and Overheating Solder.=--After solder has been re-melted a
number of times or has been overheated, its content of tin will be
reduced, and the solder will become poorer and coarser. The tin melts
earlier than the lead and, being the lighter of the two, floats over it,
and is thus fully exposed to the air, the oxidising effect of which on
heated, molten metal is extremely active. The oxidised tin forms a
dross, from which most of the tin may, however, be recovered by melting
it with powdered charcoal, which combines with the oxygen and frees the
tin. The addition of a little fresh tin is desirable.
CHAPTER III
Fluxes Used in Soft-soldering
=Why a Flux is Required.=--The great essential to successful soldering
is the chemical cleanliness of the surfaces to be united, and the proper
use of a flux. Although work may be filed or scraped perfectly bright
and clean, this is not the kind of cleanliness which is alone
sufficient; there is always in course of formation a film of oxide
present, and the duty of the flux is to dissolve this and keep any more
from forming. Then, and not until then, will the molten solder “run” and
spread over faces in the intimate contact necessary. If this vital
precaution of cleaning and fluxing is always observed, the difficulties
which many beginners experience in effective soldering will vanish.
=Variety of Fluxes.=--There are a good many fluxes employed, including
tallow (largely used for lead and pewter), resin (used for lead,
compo-pipe, and tinned metals), hydrochloric acid, diluted (for zinc and
galvanised iron), and chloride of zinc (the well-known “killed spirit”).
The last-named is the most generally used, being suitable for tinplate,
tinned iron, new zinc, copper, and brass. Sal-ammoniac is also utilised,
sometimes in conjunction with chloride of zinc. The small worker who
does but a moderate amount of soldering will find it convenient to use a
soldering paste such as “Fluxite,” which is sold in a tin, and can be
kept handy and applied to the work with a sliver of wood. “Tinol” is a
paste flux in combination with a solder.
=Preparing Zinc Chloride (“Killed Spirit”).=--Make this flux at home
from finely snipped new sheet-zinc and _pure_ hydrochloric or muriatic
acid. (This is sufficiently cheap at any working druggist’s stores, and
infinitely preferable to the contaminated oil-shop quality known as
“spirits of salt.”) Stand the acid outdoors in a stoneware crock, add
the zinc cuttings a few at a time at first, and when the first violent
ebullition moderates, put in the rest. Be sure to provide an excess of
metallic zinc, observing that a quantity remains undissolved after all
chemical action ceases. Leave the metal in the liquor for twelve hours
(covering the crock with a pane of glass), then decant and filter into a
wide-mouth glass jar of handy size. _Do not add water_ to the
concentrated zinc chloride solution; dilution is sometimes recommended,
but should never be done; the heavy, slightly syrupy, water-bright
liquor should be used as it is. The alleged “cleaning” qualities of this
chloride can scarcely be admitted to exist, and its principal function
is to shield the surfaces of the work from oxidation; this it fulfils by
the formation of a viscid glaze on the heated metal when the salt
reaches its anhydrous (waterless) condition by evaporation. The addition
of water to the flux, therefore, only uselessly prolongs the period
occupied by evaporation, and wastes heat.
Always remove all trace of flux from finished work, first by soaking in
water, and afterwards by washing with soda, soap, and water. Otherwise,
there is the risk of the work being corroded.
Special “soldering solutions,” obtainable ready prepared, should not be
used in preference to zinc chloride made as before explained or to the
well-known paste fluxes.
=Applying the Flux.=--A short heavy bottle about 3 in. or 4 in. high is
best for bench use as a flux container. It should be particularly noted
that soldering and soldering tackle should be kept as far away from
other work (and iron and steel goods and tools) as possible.
A pointed wooden stick is not a good tool for applying killed spirit,
because the acid acts on the wood, which becomes unpleasant to handle,
and the liquid does not leave the wood readily enough to place the right
quantity on the exact spot to be soldered. A galvanised iron wire is
better. Another good tool is a thin steel or iron “spit,” about 12 in.
long, and a steel knitting-needle is also excellent. Should a brush be
preferred, take a few hairs from a broom, place them in one end of a
thin metal tube, and then flatten the end with a blow from a hammer.
A brush made by hammering the ends of a short length of cane until the
fibres are like bristles is frequently used for the purpose, the handle
end being soaked in molten wax before using the cane brush the first
time.
[Illustration: Fig. 1.--Wire for Applying Flux]
A convenient method of applying liquid flux is to have a bottle with a
screw cap sprinkling top such as is often used for perfumes, and to push
a length of thick galvanised iron wire through the orifice in the
stopper, leaving about 1-1/2 in. projecting above. The lower end should
just reach the bottom of the bottle, and may be flattened and pointed.
The lead nipple is squeezed round the wire to hold it firmly, and the
projecting end bent into a ring to form a handle, as shown in Fig. 1.
The cork part should be thinned a little to render it an easy fit in the
bottle neck. The flux can be quickly applied with the wire exactly where
it is wanted, and in very small quantity; for a long seam the wire can
be run along with one dip in the solution. The fingers need not be
brought into contact with the flux; the cork will not go soft and will
not sink down owing to the lead flange supporting it.
=Flux Used on Food Containers.=--Killed spirits is objectionable as a
flux for soldering vessels intended to contain food of any kind. Not
only is this flux a poison, but it is liable to produce subsequent
rusting wherever used unless all traces of it are thoroughly removed
immediately after soldering. A good non-poisonous flux suitable for tin
boxes may be made by dissolving resin in oil. Place a quantity of
powdered resin in an iron vessel, add colza, olive, or any similar oil,
and apply gentle heat, meanwhile stirring it until the resin is
dissolved. Dissolve as much resin in the oil as possible without making
the flux too thick (when cold) to apply with a brush. One or two small
experiments will soon decide the required proportions. The resin is
really the base of the flux; but the oil is added to facilitate its
application and removal before and after the soldering process.
CHAPTER IV
Soft-soldering with the Copper Bit
=Choice between Blowpipe and Bit.=--The method of heating depends on the
size of the work, or rather the area to be soldered, and the
conveniences at the command of the worker. The soldering bit, although
so commonly used, is not necessarily the best for the beginner to use
for small work. A blowpipe flame--from a bunsen burner or a spirit
lamp--is far more convenient and neat, and its effects can be applied
and localised with the greatest precision, down to the merest pin point
of heat applied at a definite spot. The bit is chiefly useful for long
joints such as in tinplate work, and for pieces bound together to which
the bit is applied to heat up and melt solder between them. But for work
where the soldering area does not measure more than an inch or so (and
there is a vast amount of this kind), the blowpipe flame is far
preferable. It must be admitted, though, that this is a matter in which
some workmen might have two distinct opinions; and, as already remarked,
the bit is far more commonly used.
[Illustration: Fig. 2.--Soldering Bit]
[Illustration: Fig. 3.--Pivoted Soldering Bit]
=Copper Bits.=--The soldering bit or bolt (miscalled an “iron”) carries
a pointed lump of copper at the end (Fig. 2), riveted in, or
alternatively, in small sizes, screwed on to the shank. Some bits are
pivoted (see Fig. 3) to enable them to point at various angles for
dealing with difficult situations.
A home-made bit (Figs. 4 and 5) may be made by drilling and tapping a
short length of 1-1/2-in. or 2-in. square copper to receive the screwed
end of a rod of 5/16-in. iron, the copper being afterwards heated and
drawn to a point or to a blunt edge as preferred. This forms a good bit
for most ordinary purposes. An axe-head or hatchet bit is shown in Fig.
6; the copper bolt is riveted in the eye of the iron rod, the bit,
however, being free to revolve, as this is essential when making joints
in heavy lead pipe, for which purpose it is principally used. Fig. 5
represents a bit which is a combination and modification of the two
others, and it is largely used for the internal soldering of bottoms of
large drums, milk churns, etc., where great local heat is required.
[Illustration: Fig. 4.--Home-made Soldering Bit]
[Illustration: Fig. 5.--Bit for Internal Soldering, etc.]
[Illustration: Fig. 6.--Hatchet Soldering Bit]
As to the size of bit required, for ordinary small work the straight
type should not be less than 8 oz. or 10 oz. (weight of the actual
copper).
Two bits are very useful in doing a large job, as the work can then be
arranged to progress continuously, one bit heating while the other is in
use.
A bit suitable for quite light work can be easily made by drilling and
tapping a piece of copper, say 1/2 in. by 1/2 in. by 1-1/2 in. long,
either in the end or in the side, for a 3/16-in. steel rod 12 in. long,
a handle being then fitted at the other end.
In the “Tinol” telescopic soldering bit for amateurs’ use, the handle is
in three parts: (_a_) the actual wooden handle bushed with metal, and
provided with a set-screw shaped like a screw eye, and therefore easily
turned; (_b_) a steel tube which telescopes into the first part, and
which is also provided with a set-screw; and (_c_) a short rod, having
at one end a hatchet-shaped copper bit. The extreme length of the tool
is 12 in., and the length, when the parts are telescoped together, is
about 5 in.
The “Fluxite” bit is larger and heavier. It has a hollow cast-iron
handle, perforated to dissipate the heat, threaded internally at one end
to receive the screwed end of the iron stem, only 5 in. or so in length,
which at the other end screws into an adapter or holder which, in turn,
receives the screwed end of the copper bolt, itself about 4 in. long.
The bit is taken to pieces in a few moments, and is quite a workmanlike
tool.
[Illustration: Fig. 7.--Spirit-heated Bit]
=Spirit-Heated Soldering Bits.=--Bits heated by benzoline or spirit may
be made with a small barrel-shaped reservoir which also forms the
handle. One end of the reservoir is fitted with a filling cap, and from
the opposite end protrudes the tube carrying the burner. To the tube end
of the reservoir an iron clip is attached, and this secures an iron bar
which stands out over the burner head. At the end of this bar the copper
bit is attached and held either vertically or horizontally in the
flame. Tool merchants’ catalogues show a variety of such implements.
Fig. 7 illustrates one of the most elaborate of them all, the weight
complete being 2-1/4 lb. It has a polished brass container A, of 1/5
pint capacity--sufficient for 45 to 60 minutes, whence the benzoline
flows to the burner B, the flame from which heats the copper bit C. This
bit may be of any of the regular shapes, and weighs about 1/2 lb. The
position shown is that for heating the bit preparatory to soldering. The
tray D catches any drips that might occur at starting, E is the stand, F
the filler cap, G is the regulating handle, and H is the clamp that
holds the bit in place.
[Illustration: Fig. 8.--Bit attached to Blow-lamp]
[Illustration: Fig. 9.--Gas-heated Bit]
A writer in _Popular Mechanics_ has stated that the ordinary blow-lamp,
with the burner end equipped with a copper bolt (see Fig. 8), makes an
excellent soldering device. The point can be easily kept at the proper
heat, and there will be no want for hot coppers. The end of the burner
is threaded on the outside, and a hole is drilled in the copper point
and threaded to match. Small holes are drilled in the copper in the same
manner as in the burner, to make vents for the flame.
=Gas-heated Bits.=--These are largely used in factories, and are
cleanly, expeditious, safe, and convenient. The type shown by Fig. 9 is
very handy, and the illustration and description are due to F. X.
Sommers, Jun., in the _American Machinist_. A mixture of air and gas
enters the pipe at about 10 lb. pressure, or enough to give a hot, blue
flame. The part A is of cast-iron, which, on experiment, has been found
to last longer without corroding than steel, although copper would be
better. The soldering bolt B was made of steel because it kept the
correct shape point much longer than cast-iron or copper, although the
latter metal is better for transmitting the heat. The point should be
tinned before using. This form of soldering head is being used on
automatic can-soldering machines, and does the work effectively. It also
saves gas. It will heat to the correct temperature in about 1-1/2
minutes.
[Illustration: Fig. 10.--Gas-heated Bit complete]
[Illustration: Fig. 11.--Air Inlets in End of Air Chamber]
[Illustration: Fig. 12.--Section through Air Chamber and Gas-reducing
Valve]
[Illustration: Fig. 13.--Details of Cones or Needles]
A gas-heated bit invented by W. G. Ryan is shown in Figs. 10 to 13. The
actual bit A is held in a steel sheath B having a space underneath the
bit to allow the gas to pass. The sheath has a row of holes on each side
to allow the gas to come through, the flame enveloping the bit when in
use. The gas, supplied through a flexible tube, passes through the tube
that forms the handle, at the end of which is a small chamber C to admit
air, which mixes with the gas to cause it to burn atmospherically, the
supply of gas passing through a small cone valve D and thence through
the air chamber. In the air-inlet holes E at the end of the air chamber
are fitted small cones F to regulate the quantity of air. All the cones,
including the gas-valve cone, are connected rigidly together, so that
when cutting down the gas supply temporarily, the air supply is
automatically reduced, and the gas flame remains in being, although its
size is much reduced. It has been found that, in some gas-heated bits,
the cutting down of the gas seriously interferes with the proportion of
the gas and air mixture, resulting in a back-fire. The device here
described has been invented especially to obviate that trouble. To
reduce the gas supply and, with it, the air supply also, all that is
necessary is a slight forward movement of the fitting to which the cones
or needles are attached. The copper bit is kept in position by the
sheath or clip, the small bolt in which can be taken out in a moment
when special attention to the bit becomes necessary. The connection to
the flexible gas tubing is at G, while H indicates a guide and stuffing
box for the gas-valve cone or needle.
[Illustration: Fig. 14.--Gas-stove for Heating Bits]
=Stoves for Heating Soldering Bits.=--Although a copper bit may be
heated in any fire, it is better to avoid the dirt, smoke and tarry
stickiness which are often present in a coal fire. In the absence of
gas, a bright, clear coke fire or a charcoal fire should be used
whenever available. Portable oil stoves of the wickless type can also be
employed, but the ideal fuel is gas, which may be regulated at will to
give a uniform temperature. Two gas-stoves specially constructed for
copper bits are shown by Figs. 14 and 15.
[Illustration: Fig. 15.--Gas-stove for Heating Bits]
=Tinning a Bit.=--Before a bit can be used, it must be “tinned,” that
is, coated with solder in a smooth complete covering, for which
purpose--by one method, not the best, but the most general--the end is
heated to a dull red, rubbed quickly with the file on the facets, dipped
in killed spirit or “fluxite,” or rubbed against a piece of
sal-ammoniac, and then applied to a stick or lump of solder, the facets
being quickly wiped or rubbed on a piece of tinplate so as to spread the
solder evenly. When properly done, the nose of the bit is coated with a
smooth film of solder. This must always remain so, or the bit will not
act, and when it is honeycombed, or the “tinning” is present in patches,
it must be re-tinned. A bit must never be raised to a red heat
sufficient to melt the tinning. The bit does not operate well at such a
heat, because its contact makes solder too fluid and apt to run too
quickly.
When dipping a hot bit, prepared for tinning, into killed spirit, a
sharp pop, without smoke or spluttering, denotes the right temperature.
If, on withdrawing the bit, it is damp and still unclean, it had not
been heated sufficiently.
Another method of tinning may be mentioned. Into a small and clean tin
box (a 2-oz. tobacco tin about 3/4 in. deep) put some scraps of solder
and powdered resin. Heat the bit to a very dull red, quickly file up
clean on one side of the point, and then plunge into the solder and
resin and rub about; it will at once take on a coat of the alloy. A
second side of the bit may be tinned by then repeating the operation,
re-heating if necessary. The bottom of the box should be covered with
solder, which adheres easily enough, with a film of resin on top. It is
probably most convenient to tin the under side and the left-hand working
face of the bit. “Tinol” could be used in this way without admixture
with anything.
Still another method is to use a firebrick having a hollow in which the
solder and resin are placed; but the tin box plan is thought to be
better.
Undoubtedly the best method of tinning a bit is that in use by the
plumber who well knows the invaluable qualities of sal-ammoniac
(ammonium chloride) for the purpose. He has no wish to squander energy
on those vigorous rubbings of the bit--on paving-stone, bath brick,
tinplate, etc. etc., and he believes that the habit of dipping the bit
into zinc chloride is both slovenly and wasteful, for not only is this
corrosive stuff sprayed about broadcast, but the remainder is soon
rendered unfit for its purpose by contamination with copper chloride and
dirt from the fire. The outlay of a few halfpence on a sizable slab of
sal-ammoniac will keep the bit in the best condition for years, and save
hours of superfluous labour. Commercial sal-ammoniac is obtainable in
large, rugged crystals of a tough, fibrous texture. A piece weighing
upwards of 1/4 lb. can be trimmed to a roughly rectangular slab, a few
inches long and wide and about 1 in. thick; and a cavity should be
scooped in one of the flat sides to accommodate the bit.
[Illustration: Fig. 16.--Tinning Bit in Sal-ammoniac Block]
Let the bit-faces be made shapely and filed bright and the tool
thoroughly heated in a clean fire, removed, flicked free of ash, and
then held down firmly in the cavity of the sal-ammoniac block (see Fig.
16). Profuse white fumes will arise, and the surface of the salt will
fuse. Bear heavily on each facet in turn, and then melt a few beads of
solder into the cavity along with the bit, and the latter will become
brightly tinned in a moment or so. The bit should be applied to the
“ammonia block” every few heats, or as required, as the work progresses,
and flicked with a tuft of dampened cotton-waste.
The sal-ammoniac has one great disadvantage--it is deliquescent
(collecting moisture from a damp atmosphere), and its near proximity to
most metals oxidises and corrodes them. Iron and steel, particularly, it
rusts rapidly and deeply. Therefore the tools (saw and chisel) used to
shape the block must be washed, dried, warmed, and greased before they
are laid by, and the waste fragments must be carefully swept up and
disposed of. The block itself must always be kept apart from tools.
Plumbers enclose it in a sheet-lead box wrapped in a greasy rag;
amateurs may store it on a dry shelf, parcelled in waxed paper secured
by a rubber band, or in a length of motor-tyre inner tube, rolled up.
=Simple Soldering.=--Scrupulous cleanliness in everything connected with
the process of soldering is essential to success. The ordinary procedure
in making a joint is to clean the surfaces first by filing or scraping
with a scraper or a knife or a plumber’s shave-hook (Fig. 17). In some
cases, dirty metal is cleansed with dilute hydrochloric acid. With or
without preliminary heating of the work, flux is then applied to the
joint, and the heated bit is held in one hand and a stick of solder in
the other, and the stick drawn along the joint while the bit touches it
(or “drops” of solder may be transferred to the work by means of the
bit). This will cause a line of molten solder to run, and some skill and
care are necessary to get just the right amount of solder without
wasting it and allowing it to spread in a lumpy fashion beyond the
necessary area. The bit is next worked up and down the joint to spread
the solder, and by the transmitted heat to make it thoroughly penetrate
the joint. This is an outline of the process, and there is a number of
points requiring special instruction or a few words of caution.
[Illustration: Fig. 17.--Shave-hook]
Note that the work must be filed, scraped, or otherwise mechanically
cleaned, and then chemically cleaned by coating with the flux just where
the soldering is required. In heating the copper bit do not let it reach
even a dull red heat. Lightly dip it into the flux to clean the point;
then, with a small button or blob of solder resting on the work, place
the bit momentarily upon it to cause the solder to flow, and draw the
bit where the solder is required.
Many beginners try to draw along the solder with an insufficiently
heated bit. The result is a series of lumps--“putting it on with a
trowel,” as it is sometimes termed. A good joint cannot be made this
way, however much solder may be used.
Some beginners fly to the other extreme, and try to make a neat job with
a red-hot bit, which results in the solder assuming a sandy appearance
and in the work being discoloured.
Others try to solder uphill--that is, they hold or place the work in
such a way as to cause the solder to flow away from where it is
required. The correct method is to solder downhill by tilting or
inclining the work, so that the solder will always collect around and
travel with the point of the bit. This, besides facilitating the work,
makes a strong joint, and imparts a clean and neat appearance to the
job.
[Illustration: Figs. 18 and 19.--Incorrect and Correct Methods of
Holding Bit]
A common mistake is to hold the bit in a cramped and awkward way, as in
Fig. 18, the hand being twisted under the handle, the thumb being
brought to the top, and the elbow forced to the side. The correct
positions of arm and fingers are shown in Fig. 19; the elbow is held
well out from the body, and the thumb is placed directly under the
handle of the bit, forming a fulcrum over which the bit may be slightly
raised or depressed at will. This is all-important when soldering very
fusible metals such as pewter, tin, etc., on which the weight of the
copper bit should never be allowed to rest, as otherwise a hole will
suddenly be made in the work. The whole weight of the bit should be
supported and balanced on the thumb by the downward pressure of that
part of the hand close to the little finger. The worker should not for a
moment lose control of the copper bit, and control is always assured
when the thumb is underneath the handle.
There is but little strength in a butt joint with the edges of the metal
only just touching--that is, without a lap; to take the example of a
small cylinder, the body seam should have at least a 1/4-in. lap. Fig.
20 represents an example of internal grooved seam soldering, which may
be executed in the following way:--After applying the flux, place a
small button of solder inside the cylinder on the seam, rest the bit
momentarily on the solder to melt it, and then draw it gently along the
seam. The cylinder should be slightly tilted to allow of the solder
travelling with the point of the bit. The hand should avoid touching any
part of the work that comes directly into contact with the copper bit,
as otherwise the hand would be badly burned.
[Illustration: Fig. 20.--Soldering Internal Grooved Seam]
[Illustration: Fig. 21.--Soldering on Can Bottom Internally]
The method of internally soldering the bottom on a canister, etc., is
shown in Fig. 21. The bottom is held in position by gently pressing it
against (but not placing it on) the bench during the soldering process,
while the tilt of the canister and the position of the bit cause the
solder to travel with the bit.
In soldering all such articles, the soldering should be done with one
sweep of the bit, the left hand meanwhile making the necessary
revolution. This saves time and solder, and avoids the unsightly
appearance of a series of starts and stops.
In work of a larger and more substantial nature, as, for example,
galvanised or tinned iron work, the bottom of the article is first
“knocked up,” and then soldered internally. Fig. 21 represents an
example of internal soldering where the whole weight of the bit is shown
resting on the molten solder inside; this provides the local heat
required to “sweat” the solder into the four thicknesses of metal which
constitute the bottom seam; and for this work the bottoming bit shown in
Fig. 3 is often used. Pewter, lead, zinc and tin--the latter should not
be confused with tinplate--do not require sweating, on account of their
low fusibility, and any attempt even to solder them with a very hot bit
will probably end disastrously.
[Illustration: Fig. 22.--Soldering Can Externally]
Fig. 22 shows an example of external seam soldering. The method there
shown is invariably adopted for simple lap seams, although grooved seams
are similarly soldered. A grooved seam, however, should preferably be
soldered internally. The position of the worker’s elbow and thumb should
be noted, as should also the tilt of the cylinder (more pronounced in
this case than the other) in order to secure the downflow of the solder.
Sweating has already been mentioned. It should be said that one of the
easiest ways in which a beginner may make a reliable joint is to prepare
both faces of the joint by fluxing and covering with a thin film of
solder, and then pressing the two parts together with the hot bit until
the top part “floats” and then settles down. The advantage of this way
is that one can be sure of perfect application of the solder to the
joint faces, since each is dealt with first and thoroughly coated, with
no faulty patches. Sweating is also done in the flame of a bunsen burner
or blowpipe, as explained later.
=Reinforced and Filled-in Soldered Joints.=--The bottoms of square or
cylindrical vessels should, preferably, be soldered from the inside, and
“buttons” of solder may be melted to assume a stout triangular-shape
stud in the corners of the square vessels. A tinned rivet is sometimes
riveted or just placed in a corner, and sufficient solder floated over
it to strengthen the corner. Solder is always liable to run through an
improperly closed seam at the corner when external soldering is resorted
to; but in cases where this is the only practical method, a tinned rivet
may be inserted from the outside, and then soldered over. It sometimes
happens that two “raw” edges require soldering together without a lap.
Where a strong joint is required a good plan is to place a length of
tinned wire over both edges and solder the lot together. In addition to
strengthening the joint, the wire considerably improves the general
appearance. A simpler joint may be made by “skimming” the solder over
with a copper bit heated only just sufficiently to melt the solder. The
quick and skilful touch is required to perform this operation
satisfactorily; but a little practice will soon bring the necessary
proficiency. The idea is to “draw” the solder across the joint quickly,
before it has time to run through. This method is useful when soldering
thin metal goods of a lower degree of fusibility than that of the solder
employed. No preparation for filling cracks previous to soldering can be
recommended, beyond such small pieces of metal that may be afterwards
soldered over and effectively hidden. It is much better to endeavour to
produce work of such quality that this expedient is altogether
unnecessary.
=Soldering Heavy Milk Churns.=--When soldering the bottom rims on large
milk churns, sufficient heat cannot be maintained with only one
soldering bit. At least two heavy bits are required, so that one may be
getting hot while the other is in use. The rims are usually tinned
before being fixed by first pickling them in dilute hydrochloric acid,
washing, and then dipping in a bath of molten tin. When repairing and
resoldering the rims, remove all dirt and rust with a file, use a few
brushfuls of raw spirits further to assist the cleaning process, then
wash with clean water and solder in the usual way, using killed spirits
as a flux.
=Soldering Hole in Enamelled Ware.=--First scrape or file away the
enamel quite clear all round the hole, apply a little raw spirit to the
surface of the iron, and coat it with solder in the usual manner. Then
cut out a tin disc large enough to cover the hole, and solder this in,
using killed spirit as the flux.
=Soldering Leaded Lights.=--For soldering the calmes of a lead-light
window, the calmes having been fitted properly together, shave a small
round dot at the point of junction, sprinkle a little powdered resin on
the shaving, and with a copper bit or with a glazier’s iron having a
tinned face, melt a small piece of tinman’s ordinary solder on the
shaved part so that it tins to the lead and forms a round button.
=Soldering Catch on Gun-barrel.=--In soldering a catch on a gun barrel
it will first be necessary to tin both barrel and catch, and then to
wire them together, in addition binding the barrels for some distance
from each side of the catch, making the ribs secure with wedges. To melt
the solder, use heaters; these are generally made of copper with iron
handles; or iron rods can be used, the ends being made red hot and
inserted in the barrels. Cut some small slips of thin solder and place
them on each side of the catch, using powdered resin. As soon as the
solder melts, remove the heaters and cool the barrels.
[Illustration: Fig. 23.--Mouth Blowpipe]
[Illustration: Fig. 24.--Black’s Mouth Blowpipe]
[Illustration: Fig. 25.--Fletcher’s Mouth Blowpipe]
[Illustration: Fig. 26.--Section through Blowpipe Flame]
CHAPTER V
Soft-soldering with Blowpipe or Bunsen Burner
=The Mouth Blowpipe.=--Although soft-soldering is usually associated
with the use of a copper bit, quite a number of jobs can be done without
one, using instead a bunsen burner or, more generally, a mouth blowpipe,
which is an inexpensive appliance, useful for both hard and soft
soldering, and with either gas, candle, or a methylated-spirit flame.
Three shapes of mouth blowpipe are shown in Figs. 23 to 25. In a
blowpipe flame there are three cones, X, Y, Z (Fig. 26). X is a
non-luminous cone, consisting of a mixture of atmospheric air and
unburnt combustible gases (each with a low temperature); Y is a luminous
cone, composed of burning gases (carbon and carbonic acid being in
excess); and Z is a cone the oxygen in which renders it less luminous
and free from combustible materials, its temperature being exceptionally
high, especially where the cone comes in contact with the point of the
cone Y. Because of its properties, Z is termed the oxidising or outer
flame, whilst Y is known as the inner or reducing flame, because when it
is applied to some easily reducible substance--say, lead oxide--the
oxygen in the substance heated mingles with the unburnt carbon in the
cone of the flame and produces carbonic oxide, the lead being thus
separated or reduced. The blowpipe flame is one of intense heat, even
that produced by blowing a common candle being capable of melting
metallic fragments when they are supported on a bed of charcoal. The
pointed flame gives the greatest heat, and this can be produced simply
by increasing or decreasing the space between the flame and the article
to be soldered or the metal to be melted.
The particular advantage of a blowpipe is that it gives a fierce heat at
a very localised area, beyond which the solder does not run, and it
enables spots to be soldered, or parts to be unsoldered, adjusted and
re-soldered without allowing heat to stray and cause trouble at other
places. A useful little addition to the ordinary blowpipe is a small
washer soldered on near the mouth end (see Fig. 23), the object of this
being to raise this part off the bench and so keep it from contamination
with dirt, filings, etc., which are unpleasant to the lips. Sometimes
the washer is made elliptical and slightly concave to fit the lips, so
that it forms a convenient stop or steady when the blowpipe is held
between the teeth without help from either hand.
=Bunsen Burner, Spirit Lamps, etc.=--The bunsen burner is, of course,
the most convenient device for heating (when the bit is not in
question); but failing a gas supply, a spirit-lamp must be employed.
This is a small glass bottle with wick, methylated spirit being used.
Plumbers and gasfitters make use of metal tubular lamps fed with spirit
poured on cotton-wool, and having a blowpipe tube attached and coupled
up to the lips with a rubber tube; they also use wax tapers.
[Illustration: Fig. 27.--Home-made Spirit-lamp]
[Illustration: Fig. 28.--Another Home-made Spirit-lamp]
A methylated wick lamp may be easily made out of a small “self-opening”
canister, as shown in Fig. 27. The holes near the top increase the
efficiency of the flame. Another spirit soldering-lamp is shown by Fig.
28. The container for the spirit can be made about 3 in. in diameter by
about 1-1/2 in. deep, with a handle soldered on. A glance at the
illustration will explain the burner. An outer wick surrounds a piece of
tube, which itself contains another wick. The spirit in the inner tube
is vaporised by the heat from the burner when the outside wick is lit.
The spirit vapour issues from a 1/32-in. hole at A. At B a ring is
slipped over the outer wick, holding it to the central tube. By lifting
the central tube the height of the vaporising flame can be adjusted. The
vaporising tube is a piece of 3/8-in. brass tube with a 3/8-in. gas cap
screwed on the end, or a brass disc can be brazed in. The total cost
should not exceed sixpence.
[Illustration: Fig. 29.--Swivelling Gas-burner for Bench Soldering]
=Bench Blowpipes.=--The best form of gas bracket for bench use is one
having a horizontal swivelling arm, and screwed to the bench by a
flange, as shown in Fig. 29. The swivelling head is also a cock, which
shuts off the gas when the jet arm is pushed over at right angles to the
edge of the bench, as indicated, and the gas is connected by an iron or
compo pipe under the bench. A second gas tap should be arranged in the
supply to regulate the amount of gas, and for reasons of safety. A
simple device (see Fig. 30) may be made by anyone, and connected to a
rubber-pipe connecting head on the gas bracket supplying light to the
bench and workshop.
A design of gas blowpipe which leaves one hand free is shown by Fig. 31.
This enables the worker to apply the solder to the work (holding the end
of a strip against it), after it has been brought to the melting heat of
the solder. The blowpipe is arranged so that it can be held in the hand
or dropped into a hole in the bench.
=Tapers.=--Tapers for a blowpipe flame are made by untwisting cotton
rope until the threads of the individual strands are straight. These are
then dipped in melted wax made by melting two wax candles over a gas
stove in a jam jar. They are repeatedly dipped until sufficient
thickness of wax is obtained. The wax should be just sufficiently hot to
keep melted.
[Illustration: Fig. 30.--Simple Bench Burner]
[Illustration: Fig. 31.--Gas Blowpipe for Bench]
=Catching-tray for Bunsen Burner.=--The blowpipe is not essential for
some kinds of work, such as when the job can be held wholly in the flame
without causing any damage. When solder is being melted to drop on to a
surface, the plain bunsen or atmospheric flame is also sufficient,
though in this case it is well to tilt the burner over so as to prevent
the solder dropping down the tube. An elbow fitted on the top of the
tube is handy in this connection, to deflect the flame at an angle, and
Figs. 32 and 33 show this, with the addition of a tray to catch the
dripping solder which otherwise would splash on the bench and cause
untidiness. The tray is riveted to a strip of brass bent round to slip
over the outside of the elbow, and a small pin riveted into the tube
prevents the tray from falling down.
[Illustration: Fig. 34.--Section through Blowlamp for Soldering,
Brazing, etc.]
[Illustration: Figs. 32 and 33.--Bunsen Burner and Solder-catching
Tray]
=Blow Lamps.=--A soldering lamp is used sometimes in the place of a
blowpipe, and it should combine perfect security with compactness and
portability. Tool merchants’ catalogues show a number of styles. In the
lamp shown by Fig. 34, benzoline is burnt. When the lamp is in use and
the body of it is very hot, the inside pressure does not exceed
three-fifths of an atmosphere, whether the regulator R is open or almost
closed. Thus the danger of explosion, which is such a drawback to some
of the lamps that use ordinary paraffin, is avoided. The upper parts of
the lamp are subjected to great heat and therefore are packed with
asbestos, which serves as a filter and stops any impurity in the
benzoline from getting to the burner. The flame can be lowered to a
glimmer when not actually in use, thus saving the trouble of relighting.
When the lamp is to be used, the regulator R is screwed up tight; and
care must be taken to ascertain, from time to time, that the burner or
nipple C is open and perfectly clean. If this becomes obstructed, it can
be cleaned by unscrewing the tube T and passing a fine steel wire
through the hole. The lamp should be completely filled with benzoline
every time it is to be used. A little methylated spirits is poured into
the basin A, and set alight. When the apparatus has become slightly
warm, the regulator is opened gradually. To extinguish the flame, the
regulator must be screwed up tight. If any escape is observed round the
screw of the regulator, the square P should be screwed up with the key
supplied by the makers, so as to tighten the asbestos packing. The lamp
above described is only one of a great number of such appliances, but it
is fairly typical of them all. The difference between a solderer’s and a
brazer’s blowlamp is merely one of size and power.
[Illustration: Fig. 35.--Soldering Lading-can handle]
[Illustration: Fig. 36.--Soldering Lug to Lamp Bottom]
=How to Operate a Mouth Blowpipe.=--The operation of using the mouth
blowpipe does not consist in blowing intermittent and strong blasts with
the lungs, as this would soon exhaust the wind power. For very light
jobs, however, this method is sometimes adopted; but once the proper way
is discovered, the user naturally falls into the use of this method.
The proper way to keep a continuous blast is to breathe naturally
through the nose, and at the same time keep the cheeks distended by
forcing the air at sufficient pressure from the lungs. The cheeks
naturally resist the pressure, and force the air through the blowpipe.
The operation requires some practice and a clear nose passage. There is
practically no limit to the time a continuous blast can be kept up.
The blowpipe flame is produced by holding the blast end of the blowpipe
just above the wick of the taper and touching the flame; the blast then
causes a long blue flame to project. This flame is hottest at the tip,
which is slightly brown.
=Typical Blowpipe Jobs.=--Some of the photographic reproductions in this
chapter show the methods of soldering comparatively light and heavy
articles. Fig. 35 shows a lading-can handle being resoldered. As it had
broken away, the old solder remained, and the joint did not need
cleaning. It is dabbed with the killed-spirit brush, and a small piece
of solder put near the joint. The flame is first played on the parts
away from the solder to get them to the requisite heat, and as the heat
reaches the solder it melts, and flows where required. Where the solder
should be the thickest, that part of the joint is inclined downwards.
A job needing very much heat, and therefore a continuous blast for some
time, is shown by Fig. 36. A lug is shown being soldered to a heavy
brass lamp bottom. Before putting the lug in position the parts of the
joints have to be tinned. This consists of applying a film of solder. In
this case the heat is applied to the lamp bottom for several minutes,
and without loss of time the part where the lug fits is cleaned with a
fine file, the spirit brush dabbed on a piece of solder, put in
position, and the flame again applied. The solder almost immediately
flows over the cleaned portion; if it does not flow as required, the
flame is played on the solder and lamp bottom, a dab with the spirit
brush helping matters. The lug, which should have been previously
tinned, is placed in position on the lamp bottom, and with a slight
application of the flame, the solder flows and unites the parts firmly
together. It should be particularly noted that, when uniting light
articles to heavy ones, the light ones should be tinned first, and
secured to the heavier article whilst the latter is still hot.
[Illustration: Fig. 37.--Soldering Wires of Vegetable Masher]
[Illustration: Fig. 38.--Holder for Applying and Adjusting Solder]
Fig. 37 shows the wires of a vegetable masher being soldered. There is
nothing special about the job, except that the solder cannot be placed
on the joint. To effect this a piece of tin (Fig. 38) is indented at one
end, and a small hole made in the centre of the depression. The bead of
solder is placed in this depression, and held over the joint to be
soldered; the flame is then played on the joint and on the solder which
flows through the hole.
[Illustration: Fig. 39.--Brushing Solder around Dial Ring]
[Illustration: Fig. 40.--Tinning Dial Ring]
Figs. 39 and 40 show the method of tinning a brass dial ring. The ring
is filed clean and placed on a piece of asbestos board, the flame being
applied until the ring is sufficiently hot all round. A bead or two of
solder is placed on, and, as they melt, the solder is brushed round as
shown in Fig. 39 with the spirit brush, the flame being applied at
intervals to aid the flow.
[Illustration: Fig. 41.--Re-soldering Kettle Spout]
=Re-soldering Kettle Spout.=--Refixing a spout in a “tinned”
wrought-iron or copper kettle. The spout and that part of the kettle
which comes in contact with it should first of all be filed bright and
clean. Next place the spout in position, apply killed spirits, and hold
it over a bunsen flame, as in Fig. 41, until sufficient of the strip
solder is melted to flow around and sweat through to make a strong sound
joint. Should any difficulty be experienced in getting the solder to
flow readily, apply a little more flux.
=Soldering Corroded Metal.=--When the surface of metal to be soldered is
badly corroded, and it is difficult to obtain a clean, bright surface
preparatory to soldering, it should be treated to a liberal application
of raw spirits of salts (hydrochloric acid), which will soon remove the
cause of the trouble, but all traces of the acid should be washed away
with clean water before attempting the soldering. It is also a good plan
in these cases to tin the surface by repeatedly rubbing it with a hot
bit and solder, together with plenty of killed spirits, before
proceeding with the actual soldering process.
=Soldering Small Work.=--When soldering two small awkward-shaped pieces
together, they can be held in position by pressing slightly into a piece
of damp clay. When the work has several soldered joints it can be buried
in sand or covered with clay to confine the heat to the part being
operated on.
Although care should be taken to limit the solder to the area of the
joint, there are circumstances in many cases where it is difficult to
prevent some of it from straying. To clean this off, resort may be had
to the blowpipe, applying the blast and quickly wiping the surface while
the solder is in a molten state. Or it may be filed off while cold and
finished with a scraper or a knife and emery-cloth. Or if there is only
a thin film the knife or emery-cloth alone will suffice.
=Soldering Pipe Joints.=--Most joints in lead, tin and compo. pipe are
now preferably made by means of a blowlamp, or with a mouth blowpipe,
strip-solder being used. When making the joint, heat the pipe in the
immediate vicinity, and, dipping the solder in the flux, stroke it
around the pipe to form the joint.
In soldering block tin or compo. pipe with a bit, if this is too hot it
will promptly melt the pipe. This is also liable to happen with very
thin zinc. The only way to prevent this is to have the bit just hot
enough to melt the solder, and not to let it rest any length of time on
the soft metal.
[Illustration: Figs. 42 and 43.--Soldered Branch Joint on Tin or Compo.
Pipe]
In making connections with soft pipe it is better to make use of brass
couplings, and these can be soldered more easily and safely by means of
the blowpipe than with a bit. First clean and tin both ends of the
coupling, and with the bit put a little ring of solder round about 1/8
in. from the end, as shown at D in Fig. 42. Next with a penknife cut a
hole in the pipe B where the connection is wanted, a neat fit for the
end of the coupling tail A, scraping the surface of the pipe all round
the hole. Insert the coupling in the hole in a vertical position.
Sprinkle a little powdered resin round the joint, or smear it with
fluxite. Using the flame of a spirit lamp or a candle and a mouth
blowpipe, heat the upper part of the coupling, being careful not to
allow the flame to come too near the soft pipe. The solder will soon
melt, and run down into the joint (see D in Fig. 43), when the flame
must be instantly withdrawn. The same proceeding can be adopted in
soldering the other portion of the coupling into the connecting pipe. If
a vertical position is inconvenient for the coupling it can still be
soldered in that position, and afterwards twisted carefully into the
desired position. In Figs. 42 and 43, C represents a wood plug for
steadying the coupling tail.
[Illustration: Fig. 44.--Soldering Birdcage Wires]
=Soldering Birdcage Wires.=--For this job, it is better to flatten out
the solder to the thinness of brown paper and with a pair of scissors or
shears to cut it into very narrow strips. Take little pieces about 1/4
in. long, and with the fingers pinch them round the wires just above the
joints to be soldered. Touch each joint with a small quantity of killed
spirit, and apply the flame of a small blowlamp just underneath the
joint; this will cause the solder to run in the joint in an instant
(see Fig. 44). The flame is quite free from smoke, and does not
discolour the wire in the least, as the solder will run long before the
wire is red hot. Every joint may thus be neatly made. With a thin piece
of copper wire secured in a handle as illustrated, the solder may be
drawn any way desired to make special joints in awkward places, where
the point of an ordinary soldering bit could not be used.
=Sweating.=--In the preceding chapter it was shown how useful sweating
is, when accomplished with the help of the bit. In blowpipe work, also,
this method is of much utility, particularly in delicate work where
portions have to be joined up in very precise relations. After tinning
the joint faces the pieces are secured in accurate relationship with
binding wire, or by bolts or screws or other means, or a soldering clamp
is employed, having jaws which clamp the pieces and enable them to be
adjusted to the exact locations desired, and the flame then brought to
bear until the work is hot enough to cause the solder to run.
An example of the usefulness of sweating occurs in the making or
repairing of metal name plates having superimposed brass, copper, or
other metallic letters. The plate having been flattened and polished and
the letters cut out, filed and finished, the backs of the letters must
be rendered chemically clean by careful scraping, and are next “tinned”
with soft solder. The tinning may be done in several ways, but the
easiest is by the blowpipe, using resin oil as flux.
Each letter may be placed in succession on a lump of charcoal, using
plenty of the resin oil, and applying the flame of the blowpipe to the
surface while one hand holds the charcoal and the other the strip of
solder. To prepare the solder, which is sold in sheets by the pound, cut
some strips 1/3 in. wide. Take hold of one end 1 in. from the end, and
with a sharp knife scrape the surface, drawing the knife edge downwards.
Do not use the last 2 in. of the strip, as the handling of this part
makes it chemically unclean. The greater part of the solder should be
about the edges of the letters. The next operation is to solder the
letters to the brass plate. As the brass plate also must be chemically
clean, the parts where the letters are to go should be lightly scraped.
Having ruled parallel lines in order to get the letters in line, lay
each down in its proper place, and draw a pencil line round it; then
with a scraper just remove the surface of the brass where the letters
are to be soldered. A thin piece of solder is now placed underneath
each letter, and each in turn is fixed in its place and secured with a
loop of binding wire screwed up tight. Nothing now remains to be done
but to apply the blowpipe flame and resin oil, when the solder will run
underneath the letters. It is better to set the plate on some small
lumps of charcoal. When the letters appear to be set fast, remove the
plate and boil it in a solution of potash, about 1/2 lb. to 1-1/2 gal.
of water, and clean in dry sawdust. The resin oil may be made by
dissolving resin in sweet oil by gentle heat, until the oil will cause
the solder to run.
CHAPTER VI
Soldering Aluminium
It is well known to those accustomed to the art of soldering that there
is no solder which operates with aluminium in the same way that ordinary
solders operate with tinplate, copper, brass, etc. Aluminium soldering
presents so many difficulties that it has been thought desirable to
devote a separate chapter to the subject.
There is more than one reason for the difficulty encountered. Aluminium
does not alloy readily with solders at temperatures as low as other
metals require; and, secondly, aluminium alloys with lead solders only
with great difficulty, and with but a small proportion of lead at that.
Consequently, lead solders are not suitable for aluminium. Another and
even more serious reason is in respect to the refractory oxide which
forms at soldering temperatures, and which is undoubtedly responsible
for most of the trouble.
The soldering of aluminium is one of the most debated subjects in metal
working. Almost as soon as aluminium was prepared on a large scale, it
was discovered that the ordinary solders and fluxes did not answer with
it. Either pure tin or pure zinc will wet aluminium, and can, therefore,
be used as solder for it; experience shows that the tin soon falls
apart, while zinc by itself is brittle and discolours badly. The
failure of tin is due to the fact that it forms with the aluminium an
alloy that is decomposed by the action of the oxygen present in the air.
Although aluminium is popularly supposed to be non-oxidisable, really
the surface is covered with a very thin film of oxide, which prevents
solder from alloying with the metal. Aluminium when heated rapidly
oxidises. It is customary to scrape the metal before and during the
soldering; and although some workers say that it is useless to scrape
before soldering because oxidation immediately starts again, it is
obvious that a thin film is more easily penetrated than a thick one.
Often it answers to scrape with the copper bit during the soldering,
previously rubbing off the oxide with emery cloth. The work should, if
possible, be backed with asbestos, to keep up heat in the metal. To
discover whether the surface is thoroughly tinned, wipe off lightly, and
the untinned parts will then soon become apparent. If the oxide is not
scraped off beforehand, it will probably mix with the solder and form a
scum, which will make a neat flow difficult. Scum should be lightly
removed with an old knife blade. It is essential to “tin” every part to
be joined, as the solder will not take on any spot that has not been
rubbed in some way, unless previously coated.
=Solders for Aluminium.=--Hundreds of aluminium solders have been
invented, naturally all claimed to be strong and durable, the alloys
containing various metals, such as aluminium, antimony, bismuth,
cadmium, chromium, copper, lead, manganese, silver, phosphor tin, tin,
and zinc. A table of the most approved aluminium solders is here given.
Many of the best solders for aluminium contain a small proportion of
phosphor tin. A molten alloy containing phosphorus placed on aluminium
tends to absorb oxygen from the impure film as well as the surrounding
air.
COMPOSITIONS OF ALUMINIUM SOLDERS
----+------+-------+-------+----+----+------+----+------+-----
Tin | Zinc | Sil- | Alu- |Cop-|Bis-|Phos- |Cad-| Lead |Anti-
| | ver | min- |per |muth|phor |mium| |mony
| | | ium | | | Tin | | |
----+------+-------+-------+----+----+------+----+------+-----
72·5| 25 | -- | 1·5 | -- | -- | 1 | -- | -- | --
80 | 20 | -- | -- | -- | -- | -- | -- | -- | --
97 | -- | -- | -- | -- | 3 | -- | -- | -- | --
20 | -- | 10 | 70 | -- | -- | -- | -- | -- | --
90 | -- | -- | 10 | -- | -- | -- | -- | -- | --
65 | 27 | 5·75 | 2·25 | -- | -- | -- | -- | -- | --
30 | 20 | -- | -- | -- | -- | -- | 50 | -- | --
99 | -- | -- | -- | 1 | -- | -- | -- | -- | --
90 | -- | -- | -- | 9 | 1 | -- | -- | -- | --
6 | 77·5 | -- | 3·25 | -- | -- | -- | -- | 3·25 | --
-- | 90 | -- | 6 | 4 | -- | -- | -- | -- | --
-- | 80 | -- | 12 | 8 | -- | -- | -- | -- | --
-- | 80 | -- | 20 | -- | -- | -- | -- | -- | --
-- | 90 | -- | 5 | -- | -- | -- | -- | -- | 5
80 | 17 | -- | 2·25 | -- | -- | ·75 | -- | -- | --
75 | 22 | -- | 2·5 | -- | -- | ·5 | -- | -- | --
70 | 25 | -- | 3 | -- | -- | 2 | -- | -- | --
----+------+-------+-------+----+----+------+----+------+-----
In making the solders here given, it is advisable to avoid loss of the
more easily volatile of the metals by adopting the following
precautions: The aluminium is melted first, the zinc is added in small
pieces, then tin in small pieces, and lastly the phosphor tin.
Inasmuch as zinc alloys with aluminium more readily than does any of the
common metals, solders that will readily “tin” aluminium generally
contain zinc in varying proportions. The solders found most satisfactory
contain zinc, tin, aluminium, and a very small proportion of phosphor
tin; but they do not run very freely or fuse so readily as the ordinary
tin and lead solders, and it is necessary to use a higher temperature,
so high, in fact, that difficulty is found in using these solders with a
soldering bit, and it is generally necessary to use a blowlamp.
While there is no solder that allows aluminium to be soldered with the
facility and success experienced with other metals, that of Richard’s is
extensively used, and seems to have given as good results as any. It
consists of the following ingredients: Tin 29 parts zinc 11 parts,
aluminium 1 part, and 5 per cent. phosphor tin 1 part--practically the
same as that given in the last line of the table. This solder has
withstood the test of time better than many of the patented solders, and
can be used in jointing aluminium to aluminium, also aluminium to copper
or brass, and without the use of a flux. In making the solder it is
advisable to avoid loss of the more easily volatile of the metals. The
aluminium should be melted first, then the zinc, tin, and phosphor tin
in the order named.
When using phosphorus instead of phosphor tin in the making of aluminium
solder, it will first be necessary to incorporate it with the tin, for
which purpose take a length of 1-in. gas barrel, attach a screwed cap
at one end, and close the opposite end with a tin (not tin-plate) plug.
Remove the screwed cap, and, having carefully dried between blotting
paper the proper proportion of phosphorus, insert the latter in the tube
and replace the cap. Now put the plugged end of the tube into the molten
tin; this will melt the plug of tin and so allow the phosphorus to come
in contact with the molten metal. The ingot of phosphor tin formed is
afterwards alloyed with the other ingredients, as already explained.
=Fluxes for Aluminium.=--A large variety of fluxes have been tried with
more or less success, namely, borax, copper chloride, lithium chloride,
paraffin resin, sal-ammoniac, stearin, silver chloride, tin chloride,
venetian turpentine, tallow, vaseline, and zinc chloride. Stearin is
undoubtedly the most reliable of them all, but no flux is needed for
solders containing phosphorus, which is itself a flux.
=The Soldering Bit.=--The average temperature required to make a
satisfactory and thoroughly sweated joint in aluminium is from 650° F.
to 680° F., according to the size of the article. A blowpipe or blowlamp
will be of great value, and is frequently preferable to a bit. Should a
bit be used, see that it is of aluminium or nickel instead of copper,
the point and the soldered joint being kept much cleaner whilst removing
the film of oxide during the soldering operation. Another advantage is
that the point or “face” of the bit can be “tinned” with the same flux
as that which is used for the joint. More care must be taken in the
manipulation of the aluminium soldering bit owing to its lower melting
temperature than the copper and nickel bits.
=The Process of Soldering Aluminium.=--The soldering of aluminium must
be performed quickly to be satisfactory, as the metal, if not coated at
the first attempt, may be injuriously affected. “Tinning” the parts
required to be soldered first is another important factor; also the
distance of the overlap of the joints should not exceed more than 1/8
in., so as to allow the solder to flow thoroughly through; it does not
flow so readily as when soldering other metals.
In soldering large pieces, where the ordinary overlap is not allowable,
and where a butt joint would be weak, fit the pieces together as at A
(Fig. 45).
[Illustration: Fig. 45.--Aluminium Fitted Together for Soldering]
Solder always flows towards the hottest point. This tendency enables one
to direct its course under the blowpipe or blowlamp flame. A large flame
should only be employed in “heating” up the part to be soldered on large
and heavy work. With a small pointed flame directly on the solder and
the parts on which it rests, the solder will flow quickly, and leave a
smooth, even surface at completion.
Some aluminium solders now on the market are so hard that it is
necessary to heat them and the work to redness before they melt. Sheet
aluminium is easily warped by heat, and also contracts badly. If the
solder is too high in melting point, the metal must also be brought to
that point to cause proper union. If a hole is being filled in, the body
of the metal on heating expands all round and partly closes the hole;
also both the solder and the patch whilst hot are slightly expanded. In
cooling, the hole enlarges, the patch contracts, and the solder also
contracts; cracks result. The body of the work, if not exactly evenly
made, will warp, which is fatal to engine and similar work. By using a
low-heat solder (melting point, about 700° F.) these troubles should be
avoided.
=Soldering Aluminium to Copper or Brass.=--Aluminium can be readily
soldered to copper or brass with fine solder (2 parts of tin and 1 part
of lead): tin the metals, using stearin as flux previous to making the
required joint. It is essential that both the “tinning” and soldering
should be thoroughly done. Do not expect the solder to pull the joint
together, but see that the joint is kept under slight pressure until the
solder is hard, otherwise the joint will not be perfect. Many workmen
refuse to place any reliance in such joints.
Finally, it seems very likely that, at any rate as regards factory work,
the use of solder on aluminium objects will be wholly discarded in the
future in favour of fusion welding or autogenous soldering, in which
process no alloy is interposed between the surfaces to be joined.
Information on the subject is given towards the end of this book.
CHAPTER VII
Wiping Joints on Lead Pipes
Plumbers make joints in lead pipes with soft solder which, by means of
cloths, they “wipe” to the shape shown by Fig. 47.
Figs. 46 and 47 show the difference between a copper-bit or blowpipe
joint and a wiped joint.
=Plumbers’ Solder.=--As already stated, coarse, or plumbers’ wiping
solder, is made in the proportion of 2 of lead to 1 of block tin. Care
must be taken that the lead is quite pure and free from any other metal,
as zinc-adulterated solder will be difficult to use, and joints made
with it on service pipes will not be sound. In melting up scrap lead for
making solder, only sheet lead should be used, as the lead used in the
manufacture of sheets is much purer and contains a greater proportion of
pure pig lead. The scraps must be quite dry; a damp piece dropped into a
pot of molten metal may cause a serious accident, as the contents of the
pot may be blown out.
To test the quality of solder when made, heat it as for wiping a joint;
the correct temperature is determined by dropping a small piece of
newspaper into the pot, and if it quickly burns and catches alight the
solder is right for using. Next pour a small quantity on to a cold but
dry stone or cement floor. This, on cooling, should have a few spots on
the surface about the size of a threepenny-piece, and on the under side
should be bright nearly all over. Solder of this quality would, if
properly used, stand any pressure without sweating. If the solder on the
stone or cement floor looks white on both sides, or has a few small
bright spots on the under side only, it is too coarse and requires more
tin. On no account should the solder be heated to redness, as the tin
rises to the top and quickly turns to dross (see p. 11). If this should
happen to solder that is being used for service pipes, it should be
rectified by adding more tin.
[Illustration: Fig. 46 Fig. 47
Fig. 46.--Copper-bit Joint on Lead Pipe
Fig. 47.--Wiped Joint on Lead Pipe]
To purify a pot of “poisoned” solder (solder that contains zinc), melt,
stir in a handful of common sulphur or powdered brimstone until the mass
is of the constituency of wet sand, heat to the ordinary working
temperature, and carefully remove the crust that forms on the top, and
the solder will then be fit for use, except that a little tin must be
added to it. The presence of zinc in solder can be detected by the
difficulty of forming joints, the metal falling apart and working very
lumpy, and the joints when finished having a dirty grey appearance.
When plumbers’ solder is bought ready for use from the manufacturers, it
is usually in the form of casts of eight bars, weighing about 56 lb. to
the cast. The best only should be used, as cheap solder is frequently
the cause of much trouble if used on high-pressure work, and joints made
with it are never of good appearance. To test manufacturers’ solder,
wipe a joint with it, and if it is of good quality it will work easily
at a good heat, and when cleaned off with tallow and a clean rag it
should be well covered with bright spots.
Brass fittings should not be tinned by dipping into the solder pot, as
brass being an alloy of zinc and copper, the zinc may be melted into the
pot with disastrous results.
=Flux.=--The flux used is tallow, no other flux answering the purpose so
well, although mutton fat has been used as a substitute. Plumbers often
call tallow “touch,” and they frequently use it in the form of tallow
candles, the cotton wicks coming in handy for packing spindles of taps
and slides of gas pendants.
An excellent plumbers’ black, soil or smudge, can be bought in packets,
and requires only to be mixed with water before using. Ordinary black
consists of lampblack, glue, and water. The black should be first mixed
with water, afterwards adding the glue, which must have been previously
melted in a glue-pot. Simmer this for a time to remove surplus water.
Test the black on a piece of sheet lead and dry off slowly. If it chips,
add more black, but if it rubs off add glue.
The black should be made in small quantities, as it deteriorates if
kept.
[Illustration: Fig. 48.--Joints prepared for Jointing]
[Illustration: Fig. 49.--Marking-gauge for use on Pipe Ends]
Another recipe is to place in the pot 1/4 lb. of size or diluted molten
glue and a little water; gently warm until the size dissolves, but do
not boil. Mix 1/2 cub. in. of chalk ground to a fine powder with a
pennyworth of lampblack, and then with a pallet knife incorporate some
of the melted size with the mixture on a flat board or stone to form a
thin paste, after which place the whole in the pot, warm, and stir
together thoroughly. Test as before. Old and thick soil is thinned with
porter or stout, but do not add too much or the soil will become so
sticky that the solder will cling to it. A little brown sugar, or a
little stout, added to the black will make it more tenacious, and cause
it to dry with a slightly glossy surface. Some plumbers soil their
joints after they are made, with black japan or thinned Brunswick black.
But it is doubtful whether the effect is so good as when a “dead” black,
such as given by ordinary soil, is used.
=The Cloths.=--Solder cloths for underhand joints should be from 1/2 in.
to 7/8 in. wider than the joint for which they are to be used, and about
1/2 in. longer than they are wide. Most plumbers use the same cloths for
underhand and upright, but it is preferable to use a special cloth for
4-in. upright joints with the length 1 in. less than the width. For
getting up the heat of an underhand joint on a small pipe a larger cloth
may be used until the worker is sufficiently skilled in joint wiping not
to burn his fingers when using the correct size. For 3-in. joints and
upwards a large cloth must be used first to get up the heat, the wiping
cloth being kept warmed and ready for use when the heat is right. This
large cloth, as used by some plumbers, is often long enough to lay on
the worker’s arm, but this is clumsy to use when the joint to be wiped
is in a cramped position, and is liable to let the pipe get burnt, as
the metal it holds cannot be readily distributed round the joint; 8 in.
by 9 in. is a good size to practise with on the bench, and as more skill
is obtained it can be reduced to 7 in. by 7 in. A diagonal strap should
be stitched to the back to take the little finger and thumb; the
position for this can be obtained by laying the cloth face downwards and
placing the hand on it with the finger slightly spread; the wrist should
be over the right-hand corner, so that when the cloth is being used the
edge is readily kept parallel with the sides of the pipe. Branch cloths
are made from 1-1/2 in. to 2-1/2 in. wide and about half as long again
in width. These cloths should be about seven thicknesses of material,
all others being nine or ten.
White moleskin cloth is obtained from the tailor’s for making these
solder cloths, is usually 1 yd. wide, and costs about 3s. per square
yard. The usual method of making cloths is to cut a strip down the
selvedge of the material and fold up the strip till the desired size is
obtained; it can then be cut off the piece, and any odd ends left may be
used for packing a larger cloth. Another method is to cut a square piece
the required size, and then fold it three times each way. This makes a
rather clumsy cloth for small sizes, but makes a very good “blanket.”
=Horizontal or Underhand Joints.=--For making a successful wiped joint,
the ends to be joined must be a good fit and the temporary fixing must
be sufficiently strong so that the joints will not be broken in the
process of wiping. These two points should be always strictly attended
to. Service pipes should be tightly pressed home one in the other, the
cupped or female end shaved inside with a knife, but not close in as is
the case with soil or waste pipe; this allows the solder to fill up the
cavity, which effectually prevents any tendency to sweat. This principle
is followed up by some plumbers with branch joints on small size service
pipes, the male end being worked in with a twisting motion, to prevent
any solder getting into the pipes. All other pipe joints should be
closed, the female end being tightly worked in round the male end of
pipes as an extra precaution against the solder getting inside. It is a
good plan to black the inside of waste and soil pipes, so that the
solder will not adhere if any should get through when making the joint.
Fig. 50 shows the wiping of an underhand joint.
Beginners often spend a lot of time practising “rolling” underhand
joints. This is bad practice, and will be of no use in wiping fixed
joints. Little advice can be offered with regard to the actual wiping,
constant practice being the essential thing. See that the solder is at
the correct heat. This is readily found by dropping a piece of newspaper
into the pot, and, if it quickly browns, the solder is ready for use. If
the solder is used too hot it will quickly burn holes in the pipe, and
if not hot enough a heat cannot be properly worked up, and the cloth may
get torn trying to move hard metal. For underhand joints pour on
steadily with a circular motion on to the sides of the joint, and on to
the soil at the ends of the joint, until sufficient solder in a molten
condition can be brought up to cover the top of the joint with the
cloth, which is held underneath it; then pour steadily all over the
solder until it runs back again. Repeat this continuously until the
solder can be worked in a substantial body all round the joint without
any hard solder being left at the underneath edges. Give the joint a
last pour on, and wash all the solder into the cloth. Bring the solder
smartly on to the top, and quickly work it all round the joint with the
wiping cloth, using two fingers of one hand for the top and back edges,
and the index fingers of both hands for the underneath part. The top of
the joint should be roughly shaped first and the surplus metal brought
over the back to the underneath; this should be worked into the bottom
of the joint with a slight sideways motion. The extra body of metal
should be used to warm up any hard edges, the surplus being brought up
again to the top and quickly thrown off to the back.
[Illustration: Fig. 50.--Pipes Supported and Secured on Bench for Joint
Wiping]
[Illustration: Fig. 51.--Finished Wiped Joint]
=Upright Joints.=--These are more trying to the worker’s patience but
are the easier to wipe. After the pipe has been fixed in position, a
lead collar should be fixed a few inches below the joint to catch the
surplus metal. A piece of stout string tied by a half hitch round the
pipe will prevent any leakage of the solder. In working up the heat of
an upright joint, care should be taken to work steadily round the joint
so that the heat is the same throughout. After sufficient metal has been
splashed on with the splash stick and ladle, and the metal is at a
moving heat, roughly shape up the joint with the splash stick, keeping
the metal fairly high on the joint; then splash on a little more hot
metal all round. A warm cloth is now used to shape up the joint by
bringing the lower metal up to the higher part, after which start to
wipe first with the hand as far round the back of the joint as possible
and bring the surplus metal to the front, the cloth being held by the
thumb and the index and little fingers; then change the cloth to the
left hand and repeat the operation. The joint should be finished off at
the back, although if quickly done the finish off should not be
apparent. The collar must now be taken off and the solder it contains
melted with a plumber’s iron.
A plumber’s iron can be used to good purpose on these joints, especially
if they are out of doors and the weather is rough. The iron must be
heated to redness and well filed up.
[Illustration: Fig 52.--Making Upright Wiped Joint]
[Illustration: Fig. 53.--Wooden Collar or Platform to Catch Waste
Solder]
[Illustration: Fig. 54.--Lead Collar to Catch Waste Solder]
[Illustration: Fig. 55.--Pipes fully prepared for Jointing]
Where possible, all joints to be wiped in their permanent position are
sprung away from the wall and temporarily fixed with steel points made
from 1/2-in. hexagon steel about 9 in. long and drawn out to a point at
one end. In some cases, more particularly soil-pipe work, the pipes
cannot be fixed away from the wall; a hole must then be cut into the
wall about 4 in. back and about 12 in. square to allow the joint to be
properly made at the back.
=Wiped Joint between Lead and Cast-iron Pipes.=--In wiping a lead pipe
to a cast-iron pipe perhaps the best practice is to file clean the end
of the cast-iron pipe first and then coat with pure tin, sal-ammoniac
being used as a flux. The pipe then is washed to remove the
sal-ammoniac, and afterwards “retinned,” using resin and grease as a
flux. A plumber’s joint then is wiped in the usual way. It is necessary
to take great pains to make a good sound strong joint between the two
metals, but even then in the course of time (it may be only a few years)
the iron will come out of the solder. The first sign of decay will be a
red ring of iron rust showing at the end of the joint. This rust will
swell a little and cause the end of the soldering to slightly curl
outwards. Eventually the rust will creep between the solder and the iron
and destroy the adhesion of the one to the other. The joint would
eventually become a loose ring on the iron pipe, but not on the lead
pipe, as the expansion of lead and solder do not differ to any great
extent. Only those metals that alloy together can be satisfactorily
joined by soft soldering, and the solder should contain as great a
proportion as possible of the metals to be united.
The illustrations to this chapter (Figs. 46 to 55) are
self-explanatory.
CHAPTER VIII
Hard-soldering with Silver Solder
Hard-soldering is chiefly of two kinds, brazing and silver-soldering,
the former being employed for iron and steel, the solder used being
known as “spelter,” a brass alloy which can be obtained in various
degrees of fineness. For copper, brass, and nickel silver, alloys
containing silver are the best solders. In both forms of hard-soldering,
the flux is borax.
The methods of silver-soldering vary with the size of the work. A
jeweller may hold the work in his hand, on the end of a piece of binding
wire or on a square of charcoal, the heat being applied by a mouth
blowlamp from a horizontal gas jet, as already described. Larger work
demands a flame of greater intensity, and sufficient air can be supplied
only by a footblower or similar device, or, as an alternative, from the
flame of a suitable blowlamp.
=Silver Solder.=--This can be purchased at prices up to 3s. 6d. or so
per ounce in sheet form, about 1/32 in. thick. Where the solder is
melted down by the amateur, a good way to obtain the sheet form is to
turn the globule of molten metal on to the bench and to place a flat
iron on it; but the result will not be equal to a rolled ingot.
An old shop method of making silver-solder is to melt up old silver
(using current silver coinage is an expensive method of obtaining the
silver, and is said to be illegal) with some _brass_ pins, not the iron
ones so common now.
According to W. H. Jubb, two solders compulsory for silver articles that
have to be sent to assay for hallmarking are: (1) 12 parts standard
silver and 1 part brass; (2) 6 parts standard silver and 1 part brass.
No. 1 has a low melting point, and is termed “quick,” and No. 2, which
requires a higher temperature, is called “stark” (in some parts of the
country, “fine”), but the use of this term here is misleading. No. 2
should be used at the first heating and No. 1 at the second. These
should make ideal solders for beginner’s use, as the chances of burning
the work, even thin brass, are almost nil.
(3) 2 parts brass, 1 part standard silver; (4) 5 parts brass, 2 parts
standard silver. Whereas Nos. 1 and 2 are “silver solders,” Nos. 3 and 4
are termed “German silver solders,” as they are not so white and are
used on German or nickel silver (an alloy of copper and nickel). Both
Nos. 3 and 4 are good, have a comparatively low melting point, are much
less expensive than Nos. 1 and 2, and, if plenty of wet borax is used,
will “strike up” well. No. 3 is recommended.
“Standard silver” is about 95 per cent. pure silver. Old “sterling
silver” is 92·5 per cent. pure silver.
In making any of the above solders the brass and silver should be melted
together, and care should be taken to see that the metal is clean
beforehand. Where large quantities of solder are made, the metals are
scoured with emery cloth before they are put into the crucible.
=Requisites for Silver-soldering.=--For light jobs in silver-soldering
the special tools and materials required are as follow: Suitable gas jet
or other flame, mouth blowpipe, scraper, jar containing a sulphuric acid
“pickle,” piece of slate, camel-hair brush, pieces of lump borax, two
grades of silver solder, charcoal block, iron binding wire.
The pickle is made by pouring 1 part of common sulphuric acid into 20
parts of water, and its function is to remove all dirt and borax from
the metal. Silver-soldered articles should not be thrown into the pickle
until they are nearly cold, as otherwise the joints may crack, but in
the preparatory annealing (that is, softening) of plain metal, wire,
rod or tubing, the article may be put into the pickle when hot--but take
care of the splashes! Plunging hot copper or brass into cold water does
not have the effect of hardening it. Before placing a job in the pickle,
remove any iron binding, as this is immediately attacked by the acid.
Often it is advisable to heat the metal and put it “through the pickle”
before working on it, especially in the case of tubing that has been
lying by for some time and has become dirty.
For heavier work, a foot-bellows and gas blowpipe, or else a blowlamp,
are essential. An “Ætna” paraffin blowlamp with horizontal burner will
be found quite satisfactory, although, of course, if a gas supply is
available in the workshop the user will find that a foot-bellows and
blowpipe are more convenient. A blowlamp or blowpipe requires a suitable
tray or “forge” of sheet-iron in which coke and odd pieces of brick or
tile may be laid and used to pack round the object whilst the flame is
being played on the part to be soldered.
[Illustration: Figs. 56 and 57.--Clip for Holding and Applying Silver
Solder]
[Illustration: Fig. 58.--Pricker and Spatula for Consolidating Joints
and Applying Solder]
Among the smaller additional tools that will be required will be a clip
to hold the solder (Figs. 56 and 57) and a brass pricker (Fig. 58).
=Preparing the Borax Flux.=--Make up the flux on the slate by rubbing on
it a piece of the lump borax moistened with water. This paste may be
applied with the camel-hair brush to the parts to be jointed. The flux
prevents the oxidisation of the surfaces, which would resist the
amalgamation of the metals and the solder.
=The Method of Silver-soldering.=--In hard-soldering with silver solder,
first file or scrape the parts bright, and cover them and the solder
with the borax paste. Heat gently at first so as to harden the borax;
then continue to heat by blowpipe until a red heat is reached, at which
the solder will run. The secret is to blow continuously until the solder
runs, and not to stop half-way.
For soldering a silver watch case, an ordinary easy-running silver
solder, which melts at a lower heat than silver, will do. But to make
sure, shred the solder into very thin strips, and apply plenty of borax
to them as well as to the joint to be united. Use the blowpipe gently at
first so as to bake the borax, then heat the case all over almost to the
melting point of the solder, and direct the flame to the part to be
soldered until the solder runs and glistens. Cease blowing instantly,
and plunge the case into a solution of sulphuric acid 1 part and water
10 parts, to whiten it; then wash in hot water and dry in sawdust. Be
careful to remove all steel springs before soldering the case.
=Soldering Small Work with Paillons.=--These are small squares, say, 1/8
in., of sheet silver solder, made by using the snips as in Fig. 61, and
prepared by well covering with the borax paste. Each paillon is placed
in position with the tip of the brush, this job requiring a little
practice. The solder should be clean, and if not, should be made so by
passing through the fire and pickling. The work with the paillons in
position should be slowly heated by blowing the gas jet on a part of the
job farthest away from the solder; the borax will dry, and should the
solder have moved, replace it with a suitable tool or the point of the
wet camel-hair brush. The heat must not be applied too suddenly at
first, otherwise the borax will boil up and push off the pieces of
solder. The heat may be increased when the bubbling has ceased. Do not
hold the work too far away, or it will get dirty in the smoke of the
flame, or yet too near, else the gas will not be used to advantage. As
the work begins to get hot, slowly work the flame towards the joint
until the solder melts and runs into the joint. Give it now a little
extra heat to get the solder thoroughly down into the crevices, and then
let the work cool down. When nearly cold twist off the iron binding wire
and put the job into the pickle. Leave the work in the pickle about ten
minutes, when all the borax will be dissolved.
[Illustration: Fig. 59.--Section through Pipes prepared for
Silver-soldering]
[Illustration: Fig. 60.--Pipes prepared for Silver-soldering]
[Illustration: Fig. 61.--Cutting Up Silver Solder into Paillons]
=Larger Work.=--An example of silver-soldering larger work is the
joining together of two pipes, one smaller than the other. The best
course to adopt is to file or scrape the end of the smaller and the
inside of the larger (reaming and filing them if necessary) until a good
fitting joint is obtained, as in Figs. 59 and 60. A strip of solder is
then cut off, and, after the joint is well coated with borax paste, this
solder may be wound round the smaller pipe. If the joint is soldered in
a vertical position, the larger pipe should be the lower. The heat
should be conserved by laying the work in the coke and building the
same round, or, if the work is too large or the joint in an awkward part
of the pipe, a shield of tin plate or iron should be placed behind the
joint so that the flame is thrown back on to the work. Should the pipe
be attached in close proximity to the joint to a heavy piece of metal,
then warm this metal up first, otherwise all the heat will travel to
this part, and the work will take much longer to get to the proper
temperature. In all cases where one part of the joint is of heavier
substance than the other, that part should receive the greater amount of
attention from the flame.
=Quenching Silver-soldered Work.=--Many craftsmen object to the cooling
of the work by plunging it into water or pickle whilst it is hot; but no
damage or cracking of the joint occurs, it is thought, if the work is
not plunged when it is red hot or anywhere near red hot. Plunging into a
pickle certainly cracks the burnt-in borax, which can be readily removed
and the joint examined to better advantage. Many a silver-soldered
joint has been passed as quite sound when it has only been the borax
that has been stopping the interstices, and only after it has been
placed under service for some time does the faulty joint make itself
apparent.
Silver-soldering cannot be done on work that has been previously
soft-soldered unless the soft-soldered part is first cut away; but, of
course, soft-soldering can be readily accomplished after
silver-soldering or brazing so long as the work is clean and all burnt
borax is first removed.
=Removing Soldering Marks.=--Solder will run away from a part of a joint
instead of running into it when the edges of the joint have been
imperfectly cleaned preparatory to the application of flux and solder;
also, if some dirt has got into the flux, or on the paillons of solder
employed. Another cause is unequal heating of the joint, or allowing it
to expand too much whilst being heated. The resulting fire marks may be
removed by warming the articles on a pan over gas, and plunging them
whilst warm into the sulphuric acid pickle. Or the marks may be removed
in a hot and strong solution of potassium cyanide, and the polish
renewed by a light polishing with a revolving swansdown mop and rouge
composition.
CHAPTER IX
Soldering Gold and Silver Jewellery
Two methods of soldering are in common use among jewellers and
silversmiths. Soft-soldering is done with fine solder (1 of lead and 2
of tin), and is used for articles that will not bear much heating. The
metal is filed or scraped clean and bright where the solder is wanted to
run, killed spirit is applied, and a little solder is run on the
surfaces by applying gentle heat. Having thus been “tinned,” the parts
are placed together and heat applied until they unite, a spirit lamp or
a blowpipe being used. This is the sweating process, already referred to
a number of times.
For soldering catches and joints to cheap metal brooches that have been
silver-plated or gilt, the same solder is used as in the above. Both
catches and joints can be cheaply purchased, hard-soldered on to small
plates, square, oval, or crescent shaped, to suit all kinds of brooches.
Take one of these and hold it with an old pair of soldering tweezers in
the flame of a spirit lamp, and give it a coating of solder on its under
side. First wet it with the killed spirit, and then place a small
portion of solder on it, and hold it in the flame until it flows all
over the plate. It can be assisted to flow evenly by a copper wire,
which is also useful to apply the acid flux. Having “tinned” the catch,
clean (by scraping bright) the brooch, and place the catch in position.
Direct a gentle blowpipe flame to it until it is seen to settle down and
the solder flows. Then wash it immediately in warm water to remove the
acid and dry in sawdust, kept in a warm place. Use as little solder as
possible, and only clean the brooch where the solder is required to run.
Attention to these points will ensure a neat job.
Hard-soldering on jewellery, etc., is done with silver or gold solder,
and requires the articles to be heated to a bright red. The parts are
cleaned, and a paste of borax and water is applied as a flux. A small
piece of the solder is also dipped in the borax paste and laid over the
join. Gentle heat is first applied to bake the borax hard, then by the
use of a blowpipe the parts are raised to a red heat until the solder
runs. The instructions given in the preceding chapter apply generally.
With regard to gold-cased jewellery, it is useless to attempt to
hard-solder gold that has the least trace of soft solder or lead on it;
the heat causes the lead to heat into and rot the gold, and the articles
will tumble to pieces. The only way to mend, say, a gold-cased lead ring
is by soft-soldering a tin band or plate over it, applying the heat very
gently to avoid melting the lead inside.
For hard-soldering a gold ring without discolouring it, use solders
containing gold, the precious metal in the solder being afterwards laid
bare by a process of annealing and pickling. The solders are prepared
to suit the quality of the gold to be soldered, so that they may
“colour” well and thus hide the joint. The following is a list of
coloured solders:
Best solder: Fine gold, 12-1/2 parts; fine silver, 4-1/2 parts; copper,
3 parts.
Medium: Fine gold, 10 parts; fine silver, 6 parts; copper, 4 parts.
Common: Fine gold, 8-1/2 parts; fine silver, 6-1/2 parts; copper, 5
parts.
The gold solder is cast in long ingots, rolled thin and flat, and cut up
or filed into dust, and thus applied to the cleaned joints, using borax
as a flux. After the joint has been closed under a blowpipe flame, the
whole ring is annealed on an annealing plate to a dull red heat, then
cooled, pickled in acid, and polished. The film of grease left by the
polishing process is washed off in hot soda water, and the ring dried in
hot sawdust. Hard-soldered rings may be coloured with a film of
electro-deposited gold.
If the gold is of common quality, under 12-carat, to remove any excess
solder make a mixture by reducing to powder 1 oz. of green copperas and
1/2 oz. of saltpetre and boiling in 5 oz. of water. This will
crystallise when cool. Redissolve the crystals in eight times their bulk
of muriatic acid. For use, add boiling water, and place the gold in the
hot mixture. For gold of 12-carat or over, nitric acid and water (1 part
of acid to 2 of water) will dissolve the solder without injuring the
gold.
Gold solders used on gold articles are made from gold of the quality of
the article--say, 18- or 15-carats--to which is added 1/12th or more of
silver and 1/24th or more of copper. The quality of the solder is always
a trifle inferior to the metal on which it is used, so that the solder
may melt at a lower heat than the article. The melting point of 18-carat
gold is 1995° F., of 15-carat 1992°, and 9-carat 1979°, while easy
silver solder melts at about 1802° F. This shows that although 9- or
15-carat gold could be used to solder 18-carat, it is not possible to
use 18-carat to solder 15-carat. The same principle applies to silver
and brass; and the quality of the solder has to be known before any
attempt should be made to carry out the actual soldering of an article.
Another important point is that thin gold articles, like brooches, will
not bear so hard a solder as the same quality of gold will do when made
up solid, as in the case of a bangle ring. Solder for 18-carat and
15-carat is made thus: Take 1 dwt. of the gold, and add 2 gr. fine
silver and 1 gr. fine copper; melt well together, and roll out thin. For
12-carat, the addition of 3 gr. fine silver and 1 of fine copper to the
dwt. is advisable; while for 9-carat the most useful solder is made from
1 part fine gold, 1 part fine copper, and 2 parts fine silver.
Great care must be exercised in hard-soldering gem jewellery, as the
stones are likely to be injured. Diamonds are the only stones that it is
safe to heat to redness in soldering. Fancy coloured stones, such as
rubies, emeralds, sapphires, topazes, amethysts, garnets aquamarines, or
pastes must not be made hot. A ring with any of these stones may be
hard-soldered at the back if the stones are covered up with a pad of wet
tissue paper to keep them cool; but if the soldering has to be done
anywhere near the stones, they must all be taken out by un-setting.
Articles set with pearls, turquoises, opals, or cat’s-eyes (these things
are not really “stones”) will bear no heat whatever, and must all be
taken out before soldering.
In cases where it is very desirable to leave the stones in place, in
order to prevent their bursting when heat is applied to the jewellery,
cut a juicy potato into halves and make a hollow in both portions, in
which the part of the ring having jewels may fit exactly. Wrap the
jewelled portion in soft paper, place it in the hollow, and bind up the
closed potato with binding wire. Now solder with easy-flowing gold
solder, the potato being held in the hand. Another method is to fill a
small crucible with wet sand, bury the jewelled portion in the sand, and
solder in the usual way.
To restore the colour of gold or silver after soldering, dip the
articles while hot into pickling acid (1 part of sulphuric acid to 10
parts of water); or put them in a little acid in a pan and boil them in
it. Here, again, diamonds are the only stones that may be dipped hot,
and there is a slight risk even with them. Pearls, etc., must not touch
the acid, either hot or cold.
After heating and pickling, all gold is of a pale colour, and the
commoner the gold the paler. However, 18-carat gold may be restored to
its original colour in a few moments by buffing with rottenstone and oil
on a leather buff or on a brush, and following with rouge in the same
way; or it may be burnished if the nature of the article permits this.
Poorer qualities of gold may be restored to their bright colour by the
same means, but this takes longer. Most 9-carat articles are gilt to
improve their colour, and after soldering must be re-gilt to restore
their original appearance.
CHAPTER X
Brazing
Hard-soldering by brazing with spelter is used to a very great extent in
the metal industries, especially in the manufacture of cycles and
motor-cars. Although several mechanical joints have been tried in cycle
manufacture, the greatest number of joints are made by means of brazing
solder. A joint made in this manner is almost as strong as a weld, and
the steel tube itself will often break under a strain and the brazed
joint remain intact. Copper and brass tubes, when well brazed, will
stand a pressure of 40 lb. or more per square inch.
=Spelter.=--Hard brazing solder (spelter) is somewhat difficult to make.
The metals have to be melted in a crucible and cast at a proper heat,
and while in a certain condition have to be pounded or punned in a
mortar. This disintegrates the materials and forms crystals of various
sizes, some being as coarse as wheat grains, varying in fineness down to
that known as 0 0, which is very fine dust indeed, and used only on very
particular work, such as tubing 1/8 in. or 3/16 in. in diameter. The
quantity of 0 0 from 1 cwt. of solder is very small, the corresponding
quantity of coarse grains being much larger; so that unless a quantity
is required, it is cheaper to buy than to make. It is necessary to
employ the purest materials, and in purchasing hard solder it is
advisable to state the purposes for which it is to be used.
As a general rule, a solder should melt at a heat just under the melting
point of the metals to be united. Now, in ironwork, or with the steel
used in cycle work, this is impossible, for the melting points of these
two metals are too high to be effected by the bunsen blowpipe or brazing
hearth; but to join two metals in which the melting point approximates
very closely to that of the solder requires great care in order that the
metals may not be fused and the join spoiled. The reason why the melting
point of solder should be about the same as that of the metals being
joined is apparent when it is remembered that heat and cold, vibration
and concussion, tension and compression, have very considerable effect
on metals, and that if the expansion and contraction of these under
working conditions is not nearly alike, disruption or opening of the
joint will follow.
Hard solders or spelters are mainly composed of copper and zinc--that
is, they are brass alloy--the quality most extensively used consisting
of equal parts of copper and zinc. As the quantity of copper in the
solder is increased, so the fusing or melting point is raised.
Ordinary copper melts at about 2,000° F. and zinc at about 840° F., and
a solder composed of equal parts of each metal has therefore a high
melting-point.
A very hard solder consists of equal parts of silver and copper.
Generally, a spelter of different composition is required for iron,
copper, and brass work, that for the latter being required more readily
fusible than that for the former. A suitable spelter for ironwork is one
composed of 2 parts copper and 1 part zinc; a spelter for copper
consists of 3 parts copper and 2 parts zinc; while equal parts of copper
and zinc make a suitable spelter for ordinary brass work. If a very low
melting point be required, a little silver should be added to the
last-given spelter.
=The Flux.=--Borax is the best-known flux for brazing. It is beneficial,
however, to have the borax calcined (fused), as it settles down to its
work immediately when applied to the hot metal, whereas uncalcined borax
has a tendency to swell and fall off the work.
Spelter is in the form of filings, a thin stick, or wire. Filings are
apt to be blown from the work. Brazing is a very useful, and, if
properly done, reliable, method of joining two pieces of iron. A brazed
joint is considerably stronger than a soft-soldered one, and easily
resists temperatures that would cause ordinary solder to run.
The process is not at all difficult if there is sufficient heat, and,
for those who have no gas laid on, the purchase of a paraffin Ætna
brazing lamp can be recommended. With this lamp, of course, the bellows
is not used, and only an iron hearth with asbestos cubes is wanted; but
gas should be used if available.
=The Method.=--For satisfactory brazing, thoroughly clean the surfaces
to be joined, first with a file and then with emery-cloth, and, if
necessary, bind them together with thin iron wire. A flux of borax and
water mixed up into a thick paste is smeared round the joint, which
should then be warmed to get rid of the moisture. Heat the metal to a
white heat, dip the spelter into the borax paste, and apply to the part
to be joined, rubbing round the joint until the brass is seen to run,
when the heat can be cut off. The work should be almost covered in the
asbestos cubes, and the spelter applied all round and not only in one
place; failures to unite the parts mostly result from insufficient heat
or cleaning of the parts.
=Brazing-lamps.=--These lamps are constructed to burn benzoline or
paraffin, and the more powerful types are fitted with pumps so that air
pressure may be exerted on the oil. The paraffin or benzoline is thus
forced into the burner, and by passing through the previously heated
tubular coil is converted into gas, which issues forth out of the gas
nipple, mixes with air, and then burns with a blue atmospheric flame of
high temperature. After filling the lamp, a torch should be held under
the burner to vaporise the oil, and thus ignite the lamp, after which
pressure is applied by means of the pump. Do not start pumping too
soon--that is, before the burner is sufficiently hot to vaporise the
oil--or the oil itself will be forced through the gas nipple. The flame
may be regulated at will, to suit the work in hand, after the burner has
become thoroughly hot to set the lamp fairly going. When brazing, lay
the article to be brazed on some broken coke, charcoal, or firebrick,
and if the article is comparatively heavy, cover it over with some small
pieces (to conserve the heat) except where the brazing is required.
After applying flux and spelter to the previously cleaned metal, direct
the flame of the lamp on it, gently at first, until the spelter fuses
and makes the joint.
=Gas Blowpipe for Brazing.=--Brazing blowpipes should be fitted with a
combination air and gas regulator, by means of which both the size and
nature of the flame can be adjusted to suit the work in hand. When
choosing a blowpipe it is always better to make one rather larger than
the work in hand necessitates--the flame can be reduced when required;
by this means a margin of reserve is provided which is useful in
emergencies. A blowpipe whose dimensions are 10 in. long, having a
5/8-in. gas supply reduced to 7/16 in. at the nozzle, and a 3/8-in. air
supply reduced to 3/16 in. at the nozzle, will braze ordinary latch keys
and other similar work if used with a No. 3 size blower. As already
stated, a paraffin, petrol or benzoline blowlamp is a cheap and
effective apparatus, especially where the quantity of work to be done
does not warrant the outlay of a foot blower, gas blowpipe, etc., but
gas has advantages over the liquid fuel, inasmuch as the blowpipe is
more under control. The quantities of gas and air can be readily and
more delicately adjusted during the actual brazing process, then as soon
as the spelter fuses and the gas is turned off, the stream of cold air
soon counteracts any excessive heat.
=Making a Gas Brazing Hearth.=--The brazing hearth can be bought
ready-made, or can be cheaply put together by the worker himself, the
necessary materials consisting of two bel
Cite this
"Soldering, Brazing and Welding". Project Gutenberg. Public domain in the USA. https://www.gutenberg.org/ebooks/52074 JSON record · API collection · BibTeX · RIS · CSL-JSON · citation policy