The Royal Mint
796,272 chars · English
The Project Gutenberg eBook of The Royal Mint
This eBook is for the use of anyone anywhere in the United States and
most other parts of the world at no cost and with almost no restrictions
whatsoever. You may copy it, give it away or re-use it under the terms
of the Project Gutenberg License included with this eBook or online
at www.gutenberg.org. If you are not located in the United States,
you will have to check the laws of the country where you are located
before using this eBook.
Title: The Royal Mint
its working, conduct, and operations, fully and practically explained
Author: George Frederick Ansell
Release date: May 24, 2026 [eBook #78741]
Language: English
Original publication: London: Effingham Wilson, 1871
Other information and formats: www.gutenberg.org/ebooks/78741
Credits: deaurider and the Online Distributed Proofreading Team at https://www.pgdp.net (This file was produced from images generously made available by The Internet Archive)
*** START OF THE PROJECT GUTENBERG EBOOK THE ROYAL MINT ***
Transcriber’s Notes:
Underscores “_” before and after a word or phrase indicate _italics_
in the original text.
Equal signs “=” before and after a word or phrase indicate =bold=
in the original text.
Small capitals have been converted to SOLID capitals.
Footnotes and illustrations have been moved so they do not break up
paragraphs.
Deprecated spellings have been preserved.
Typographical and punctuation errors have been silently corrected.
THE ROYAL MINT:
_=Its Working, Conduct, and Operations,
Fully and Practically Explained;=_
WITH
SUGGESTIONS FOR ITS BETTER SCIENTIFIC AND OFFICIAL MANAGEMENT.
RE-WRITTEN, ENLARGED, AND REVISED TO THE PRESENT TIME.
TO WHICH IS ADDED, AS AN APPENDIX,
A LETTER ADDRESSED TO THE RIGHT HON. LORD KINNAIRD, K.T.
BY GEORGE FREDERICK ANSELL,
ANALYTICAL CHEMIST.
LATE OF THE ROYAL MINT,
FORMERLY OF THE ROYAL COLLEGE OF CHEMISTRY.
_ILLUSTRATED WITH ENGRAVINGS._
“To have a thing is little if you’re not allowed to show it;
And to know a thing is nothing unless others know you know it.”
LORD NEAVES.
THIRD EDITION.
[Illustration]
LONDON:
EFFINGHAM WILSON, ROYAL EXCHANGE.
1871.
_Entered at Stationers’ Hall._] [_All rights reserved._
Ipswich, _March 1st, 1871_.
DEAR MR. ANSELL,
I have no objection to your appending to the third edition of your book
your letter to me in regard to your case, and my correspondence with
Mr. Gladstone and the Chancellor of the Exchequer, but if you add in
addition to this correspondence the report of the debate on my motion
for a committee to inquire into the management of the Mint, I should
wish to make some few remarks on the subject in question; but before
doing so I must take the opportunity of thanking you for letting me see
Mr. Fremantle’s letter in answer to your offer, made at my suggestion,
to meet Mr. Fremantle with a view to rendering him some assistance
(which from your great experience you are well able to do) in the
management of the Mint, which I have reason to know both he and Mr.
Lowe find _somewhat difficult_.
The answer is evidently dictated by Mr. Lowe. After his letter[1] to
me of the 29th April, 1869, I might have known that he was not likely
to do anything which might appear as if he owned himself in the wrong.
This letter, indeed, showed how annoyed Mr. Lowe was at my having seen
that most malicious report to the Treasury by Dr. Graham, which has
been the cause of your having been so unjustly dealt with, to the ruin,
in a great measure, of your prospects in life. Dr. Lyon Playfair at the
time threatened that if I moved to inquire into the management of the
Mint, he would move that that report be laid on the table of the House.
This would not have deterred me, as the report _itself_ would have been
the best refutation of the _insinuation_ it contained that you were
dismissed because you were guilty of the Mint practice of purloining
gold (whereas the note[2] relieving you from further attendance stated
that the short work at the Mint was the cause). Dr. Graham did not,
he said, believe the insinuation, and to show that he did not believe
it, although he had sent in the report to the Treasury, he authorised
me to offer you the situation (at an increased salary) filled by Mr.
Goodwin, who was to be retired, which of course you refused as being
far inferior to the one you held; and in further proof he wrote you
that handsome testimonial[3] which I read to the House of Lords.
[Footnote 1: See page 196.]
[Footnote 2: See page 186.]
[Footnote 3: See page 198.]
The report, however, _had served its purpose_ in preventing you from
being appointed to an office in the Mint.
I am sure Dr. Graham regretted that he had been induced by his brother,
whose animus against you was known throughout the Mint, to send in such
a report to the Treasury. Dr. Lyon Playfair’s threat, as I have said,
would not have deterred me from moving for a committee to inquire into
the malpractices of the Mint, but I confess that I had great scruples
in regard to Dr. Graham himself. I shall never forget the expression of
his face, and the fearful agitation the mention of my intention always
caused.
I confess I did hesitate to place a man of Dr. Graham’s great
scientific attainments in such a position as an inquiry would have
done, seeing also that his brother was just dead, and that I knew
individually Dr. Graham was in no way implicated in the malpractices
which formerly prevailed in the Mint; for, as you know, Dr. Graham
had soon after his appointment set to work to clear out that “Augean
stable,” which, with your assistance, he had almost accomplished till
in an evil moment he appointed his brother, to whose intemperate habits
I referred in the House of Lords,[4] to a responsible office in the
Mint.
Dr. Graham’s death following so soon after that of his brother, I was
greatly rejoiced at having delayed bringing the subject of the Mint
before Parliament, because I should have felt that I had been to some
extent instrumental in hastening that event by drawing attention to the
state of that Department.
On the occasion of the reading to me, by Dr. Lyon Playfair, of that
wicked report to the Treasury (to which I have previously alluded),
in the presence of Dr. Graham and of Mr. C. W. Fremantle, I urged, as
Dr. Graham exculpated you from all blame _insinuated_ by the report,
that in common justice you should be reinstated in some office in the
Mint, you having, with my advice, refused the position offered by Dr.
Graham through me, when Mr. Fremantle remarked as a reason against
your being appointed that “you were so unpopular with the officials;”
such unpopularity being in my opinion the natural result of the work
you had done at the request of Dr. Graham, and in the service of the
Mint. I say the work you had done, and use the expression on the
authority of Dr. Graham, copies of whose letters to the Treasury are
now in my possession, and in which he distinctly states that to you
mostly were due the reforms. There is no doubt, therefore, but that
you were exceedingly unpopular just in the sense that a detective
would be amongst the “light-fingered gentry,” and had I obtained the
committee for which I moved I could have shown the true grounds of
your unpopularity. I have collected some further valuable information
showing the necessity for a rigid and full inquiry into the affairs of
the Mint, which will show that the officials of a public department
are not justified in putting into the hands of a young and rising
member of the House of Lords statements which are not only erroneous,
but absolutely false, so that Lord Lansdowne was obliged to declare
that “he had on a previous occasion overstated the amount in regard to
the profit on silver;”[5] but again was he grossly misled by the Mint
officials when he stated “that there was a gain of £5,000 per annum
on the silver coinage”[6] (a considerable reduction on the former
statement) while the _return_ showed a positive and very great loss. It
would appear that the Mint officials mystify him, and that _he_, not
_I_, confuse two things.
[Footnote 4: See page 197.]
[Footnote 5: See page 146-148.]
[Footnote 6: See page 148-149.]
I alluded in the House to a job by Mr. Lowe in appointing Mr. Roberts,
and Lord Lansdowne in reply stated that Mr. Roberts was a _very eminent
chemist_ who had proved his capability by “_devising_ a system for
depriving brittle gold of the obnoxious properties on which I recently
commented.” Have you heard that the plan has been tried and found to
be a complete failure!!! I am also informed that Mr. Roberts _did
not devise_ the process in question, but that it was invented by a
really eminent chemist, who did not make the inquiry with a view to
its application under the circumstances which arise in the Mint, where
operations are conducted on so large a scale. The process is described
in the British Association Reports for 1848, and more fully in the
_Philosophical Magazine_ for 1850.
I have just received the Report of the Deputy-Master of the Mint, on
European Mints, which I have only had time to glance over. The report
is evidently framed with a view of meeting the allegations I made on
the appointment of the commission. It would appear, moreover, that Mr.
Fremantle and his colleagues have made a _very careful study of your
book_!!! which might have been done without the pleasant trip. For
the general public the reports are interesting as showing how foreign
mints are worked, but as far as the management of the English Mint
is concerned, and how a department which is a serious expense to the
country, and from which no one but the Bank of England and the employés
derive any profit, can be made, as it ought to be, a source of revenue,
the report does not show. I see it is proposed to build new offices,
“so constructed as to diminish facilities for peculation!!” I think
the real question is, would it not be better TO COIN BY CONTRACT—this
might be tried, at all events for a time, before the new offices are
commenced.
I almost fear this Mint question will not be taken up in the House
of Commons, as members are afraid to “tackle” Mr. Lowe, and in these
fearfully excited times the subject is _too dry_ for members to
interest themselves in; but I cannot understand how a Government bent
on economy and reforming abuses in the several Departments can allow
such wasteful extravagance and useless losses to go on, unless indeed
Mr. Lowe is dreaded as much at the Council Board as in the House of
Commons.
Believe me,
Dear Mr. Ansell,
Yours faithfully,
(Signed) KINNAIRD.
To G. F. Ansell, Esq.,
27, Bernard Street, Russell Square, London, W.C.
PREFACE TO THIRD EDITION.
Influential friends have advised me to issue the present as the
_third_ edition of “The Royal Mint” on the ground that a Treatise on
Coining which I wrote, at the request of Mr. Graham, for “Tomlinson’s
Cyclopædia,” of which Mr. Tomlinson allowed me to have a hundred copies
printed and bound separately for private circulation, was really the
first edition of the more extended work I have recently published. The
copies of that first edition were soon absorbed: indeed, owing to the
fact that there is little literature in relation to the Royal Mint, I
was flattered by foreign governments and foreign mints seeking from me
copies of that book. Such applications gave me pleasure, and as far as
I was able I complied with the requests preferred, except in the case
of the Spanish mint, for which institution Mr. Graham asked of me a
copy when, unfortunately, I had parted with the last at my disposal.
I was further gratified by the fact that the Imperial Government of
France sought permission to translate this book into French, with a
view to give a copy to each workman in the mints of that nation.
Under considerable pressure I re-wrote the book above spoken of for
public use, but omitted to style it, as I should have done, the
_second_ edition. This, in its turn, was most kindly received by those
whose opinions I value in both Houses of Parliament, as well as by
those who understand in an especial degree the subject of which I
treated; and I have reason to know that it has found its way to all,
even the most distant, parts of the world. It was produced, but not
replied to, by Ministers in both Houses of Parliament, and remains
yet uncontradicted (see page 198); indeed, I may assume that it has
been officially confirmed; for on the motion of the Right Honourable
Lord Kinnaird, returns were made to the House of Lords, which are
verbatim copies of some of the most damaging pages in my book up to and
inclusive of the dates then reached (see pages 91, 97, 102, 133, 135,
197-8). I say thus much in gratitude, for the subject I have chosen is
one which could hardly have induced me to expect for it so generous
a reception. I wrote it hoping only that the public would acquaint
themselves with the manner in which one of the principal Departments
of the Government was and is conducted. Lord Kinnaird, in the letter
which he has done me the honour to write, and permits me to print in
these pages, expresses an opinion—one that is largely entertained—that
Mr. Fremantle and his fellow-travellers to European mints are greatly
indebted to my books for the information on which they found their
opinions, as expressed in the reports on foreign mints. For their own
sakes as well as for the benefit of the nation, I would that those
gentlemen had followed in their entirety my suggestions, because such
a course would have enabled them to avoid those difficulties which
beset them, and pitfalls into which they will stumble in the carrying
out the designs expressed in these reports on European mints; these I
will discuss in the fitting place, but here I desire to thank those
gentlemen for such attention as they have given to my opinions.
The leading newspapers and periodicals have reviewed or noticed the
books in a kindly spirit, with but one exception, in which the writer
without refuting one statement indulged in personalities. To those
gentlemen of the Press who have spoken candidly and generously, I offer
my best thanks. I have endeavoured to correct the faults they pointed
out—unless, indeed, where principle was concerned; and, in deference
to the expressed opinions of some of my reviewers, I, now that a new
edition is called for, publish, by his Lordship’s authority, a letter
which I wrote to Lord Kinnaird at his Lordship’s request, giving a
history of my dissociation from the Mint, in which, I hope, will be
found evidence confirming the statements I make throughout the book.
I do not attempt to disguise the fact that I consider myself to have
been seriously wronged both by Mr. Thomas Graham and by the Treasury,
still I consider, wisely or unwisely, that my personal grievances are
of less interest to the public than is the principle involved. I,
however, deem it right to invite attention now to the subject of my
complaint,—fully set forth in the Appendix,—because it is illustrative
of the treatment a public servant will surely receive if he should
follow the intimation conveyed by the present Government, and,
neglecting the fact of his own relative position, fulfil the duties of
his office as he would do if the matter in hand were one of personal
concern. The Government of the Right Honourable W. E. Gladstone, from
their bench in the House of Commons, promised that “if each in his
especial sphere would faithfully fulfil the duties required in his
department irrespective of his nominal position,” “such public servant
should be duly rewarded:”—the Ministers might have added, and would
have so added had they been candid, “with immediate discomfort and by
ultimate dismissal, and that justice would be sought at _their_ hands
by such public servant in vain!”
The effect of a rule which obliges Ministers to support the “head of
a Department” “_under any and all circumstances_,” will be apparent
to all evenly balanced minds; and I from my own knowledge, without
fear of contradiction—except, indeed, official denial, which is now
so perfectly understood—state that the man who best succeeds in a
Government office is he who does unreasoningly and undoubtingly just
what he is told to do, and avoids giving offence to his superior
officers by pointing out any irregularity or improvement.
Upon the publication by Mr. Thomas Graham of the malevolent report he
had written to the Treasury, I, when that fact was made known to me,
obtained a high opinion, and in pursuance of advice then given, it was
my intention to proceed by action at law against Mr. Graham for libel,
but his early death made that step impossible.
With regard to the publication of the correspondence, it is right that
I should say that Lord Kinnaird had not intended to draw attention to
my case; but, when his Lordship found that the Marquess of Lansdowne
and His Grace the Duke of Argyll led off against me in the House of
Lords, as the Right Honourable Robert Lowe had done most bitterly in
the House of Commons on the previous Friday, he with great generosity
threw off the natural reluctance he had entertained to hurting the
feelings of Mr. Graham’s friends, and defended me with words and
documents so nobly that I can never sufficiently thank his Lordship, or
fittingly acknowledge the indebtedness I thereby incurred.
To Mr. Lowe, Lord Lansdowne, and the Duke of Argyll must be attributed
any pain which may arise to the friends of Mr. Graham, for Lord
Kinnaird desired to spare them; for myself, however, I would say
that if either of the Ministers named had obligingly pointed out any
presumedly false statement contained in the book which has so far
excited their anger, and proved its untruthfulness, instead of saying
hard words of the Author, I should have been less mindful of the sage
instructions given on a celebrated occasion to an eminent Advocate, “It
is a weak case, bully the counsel.”
Some of my readers will perhaps consider that the following pages
are overlaid with a strong personal feeling, and may therefore feel
disposed to lay the book aside. To such I would remark that it is
impossible to follow a pursuit of any kind earnestly, unless it be
made a matter of undivided interest. Besides, it must not be forgotten
that I was invited to go to the Mint solely on the ground of my known
determination to resist abuses. Having devoted fifteen years to the
subject of the Mint, it is not to be supposed that I can view its
mismanagement with less concern now than I did when selected for
appointment to that Department, that I might repress irregularities
which were then known to exist, and which appear to have been as yet
uneradicated.
With such remarks, I invite a perusal of my new edition by such members
of the legislature as are really desirous of reforming the abuses which
exist in the Royal Mint.
PREFATORY LETTER TO THE FIRST EDITION.
TO
THOMAS GRAHAM, ESQ., F.R.S.,
MASTER OF THE MINT, ETC. ETC.
SIR,
I have written a short article for “Tomlinson’s Cyclopædia,” for the
purpose of explaining (as far as the limited space at my disposal would
allow) some of the details of the process of Coining, and by permission
of Mr. Tomlinson I am allowed to have a few copies of that article
printed separately for private circulation.
I take advantage of this opportunity to acknowledge most gratefully
that the information I have been so fortunate as to obtain on the
subject of Coining has been gained in consequence of the opportunities
you have afforded me in my position in the Royal Mint. With heart-felt
thanks for the privileges you have accorded me, and for the support you
have given me,
I beg to remain, Sir,
Your most faithful servant,
GEO. F. ANSELL.
ROYAL MINT, _August, 1862_.
PREFATORY LETTER TO THE SECOND EDITION.
27, Bernard Street, Russell Square, London, W.C.,
_November 8th, 1869_.
MY LORD,
I have ventured to ask permission to dedicate this book to your
Lordship, as a mark of my sense of the great kindnesses you have been
pleased to show to me through a series of years. As you, my Lord, will
perhaps permit me to remind you, generous efforts have been made by
many with a view to reinstate me in a position of which they and you
consider me to have been unjustly deprived—an opinion, I believe, your
Lordship has formed from a knowledge of all the facts.
The recent death of Mr. Thomas Graham puts an end to any personal
feeling between him and myself, whoever was right or whoever was wrong,
or even if there were faults on both sides, the matters which caused
a severance are better forgotten—our differences are beyond human
adjustment.
The information I have attempted to give in the following pages is
given solely with a view to throw as much light as is possible upon a
subject which is now attracting very considerable attention, and which
has become of national importance.
It will be to me a great pleasure if I may thus express the gratitude
I feel for the valuable assistance I have received from your Lordship
during a time of great trial and anxiety.
I have the honour to be,
My Lord,
Your Lordship’s most faithfully obliged and humble servant,
GEORGE F. ANSELL.
To the Right Hon. Lord Kinnaird, K.T., F.R.G.S.,
Lord-Lieutenant of Perthshire, &c. &c. &c.
PREFACE TO SECOND EDITION.
Perhaps it will be well that I should give a brief outline of the
circumstances antecedent to and attending my association with the
Royal Mint, because the facts and opinions which will be given in the
following pages appear to require such a notice, that their worth or
worthlessness may be estimated at its true value, as well as that the
sources of my information, and the modes of obtaining it, may be in the
hands of my readers.
In the early part of the year 1856 the Master of the Mint found himself
so beset with difficulties arising from irregularities committed by
those who should have supported him, that he formed a determination to
engage a person who should be indisputably a faithful and intelligent
officer in the Coining Department, and who at the same time had
sufficient personal influence to check those irregularities which he
knew were taking place, but which were beyond his personal supervision.
These irregularities were known to the Government of that period, and
had caused so vast an expense that that Government, which was presided
over by Lord Palmerston, had intimated to the Master, that unless
the Mint could be conducted more satisfactorily and economically, it
would be broken up as an Imperial establishment, and thus necessitate
the placing of the coinage in the hands of contractors. With this
view papers were printed and issued to various firms; but Mr. Graham,
being very sincere and energetic in his desire to so conduct the
Mint as that this necessity should not arise, sought the advice of
engineers and others, with a view to finding such a man as combined
within himself the qualities which he saw to be necessary. Finally,
by the advice of Dr. A. W. Hofmann, he called upon me at my residence
in October, 1856, and related to me in detail the facts above alluded
to, and explained precisely the position of affairs at the Mint,
giving me the names of the troublesome persons, and showing his own
position to be so intolerable, that without some one on whom he could
rely, it would be impossible for him to continue his Mastership. Mr.
Graham then proceeded to tell me what had passed between Dr. Hofmann
and himself as to my fitness for the work required, and explained
clearly the impossibility of placing me in a secure position or in high
office at first, but that if I would accept a supernumerary clerkship
temporarily, he would, when I had effected the object of his desires,
advise my promotion to the office then held by Mr. W. T. Brande, when
that office should become vacant. With this understanding I agreed
to accept the position proposed if duly appointed; but that I might
be able to carry out such reforms as were necessary, I insisted on
sufficient power being given to me by himself or by the Government. In
pursuance of this agreement, Mr. Graham recommended my appointment in
a letter to the Treasury, dated 29th October, 1856, in the following
terms:—
“I desired to introduce a young man, recommended by scientific and
technical information available in coining, by energy of character,
and by tried ability in the supervision of workmen—a faculty by no
means common. After applying to Mr. William Fairbairn and to Mr. George
Rennie, who both recommended candidates, and making inquiry in various
other quarters, I have been led to propose the name of Mr. George
Frederick Ansell as temporary clerk. Mr. Ansell was educated under Dr.
Hofmann, and acted for some years as his laboratory assistant. He has
since been Scientific Director in the Panopticon, Leicester Square,
which was lately broken up. He appears to be a person of superior
education and ability, and great activity and vigour of character, and,
as I have been assured, has shown much discretion in the management of
both pupils and workmen.”
In accordance with this recommendation I was appointed to a
supernumerary clerkship, and took office in the Rolling Room of
the Royal Mint; but before doing so I particularly inquired of Mr.
Graham, in the presence of Mr. W. H. Barton, the then Deputy-Master,
what authority I should have, and how far I should be supported if I
attempted to enforce obedience, and whether I was at liberty to call
for statements and examine original documents and books. He verbally
authorised me to examine such books as I wished to examine, and desired
Mr. Barton to give me such statements or information as I might ask
for; and as to my authority, he said, “If you order the men to dance
a hornpipe on the table, they shall do it, and all orders shall pass
through your hands.” With such power, and a salary of £120 a year, or
rather £10 a month, I took office on the 12th November, 1856.
My personal experience of men and manners in the Mint is recorded
in another book, but in this I feel it right to adhere rigidly to
explanations of the processes of coining, and to treat of the expense
and loss attending the manipulation of the precious metals; and in the
latter pages I will demonstrate what formerly was, and what should be,
the cost of producing a coined sovereign, each statement being the
result of actual experience, and capable of proof.
THE ROYAL MINT.
Coining is the term applied to the processes employed in the
manufacture of money. It is proposed to describe the present mode of
manufacture; but it may be as well to state, that in remote periods
money was made by cutting out a piece of metal somewhat of the form
of the intended coin, and imparting the device to it by the blow of a
sledge-hammer. For this purpose the blank piece of metal was laid upon
a die, say the obverse, fixed into a block of wood or stone, supposed
to have been so large as to absorb the vibration caused by the blow,
and to a great extent prevent the quivering which would naturally
arise, and cause unsteadiness. The workman then took the other die, say
the reverse, and passing it through a folded sheet of lead, in order to
avoid the shock to the hand, he placed the engraved part on the blank,
which was resting on the lower die, and held it firmly while another
workman struck it with a sledge-hammer. It is worthy of remark that a
piece of lead such as that described is in the Museum of Dies at the
Royal Mint; and although its surface, by the action of the atmosphere
and other causes, is now converted into carbonate of lead, indentations
caused by the tips of the workman’s fingers are evident. This piece is
believed to have been used with a die of Edward IV. At a later period
the upper die was held in a twisted hazel stick. After each blow the
dies were what is technically termed locked together; that is, the
lower and upper dies were made to fit into the partly-formed coin, so
that neither die could turn without turning the whole mass, and then
a second or third blow was given, till the coin was completed. An
improvement on this method was effected by fitting the two dies into
rods of iron, which may be represented as a pair of tongs; the flat
parts which are used to take a coal would then be the position occupied
by the dies. This plan saved the operator some risk of bruised fingers,
but the process was essentially the same as the original one; and to
money produced by either means was applied the term _hammered_ money,
in contradistinction to _milled_ money; that is, money which was made
from blanks obtained from fillets which had been rolled in a very rough
kind of rolling mill, driven by horse power—the germ from which sprang
the present machinery. On this point it is perhaps of interest to quote
a passage from the Report made to the Lords of the Treasury in 1695 by
Mr. William Lowndes, who says:—“All the moneys we have now in England,
both gold and silver, are reducible to two sorts, one stamped with the
hammer, and the other pressed with an engine called the mill. The gold
or silver of the hammered money is first cast from the melting-pot into
long bars, those bars are cut with shears into several square pieces of
exact weight for sovereigns, angels, crowns, half-crowns, shillings,
&c. Then with tongs and hammer they are forged into a round shape,
after which they are blanched (that is, made white or refulgent by
nealing or boiling), and afterwards stampt or impressed with an hammer
to make them perfect money. This method of making money with the hammer
(as appears in the said red book) was practised in the reign of King
Edward the first” [the book referred to is in the Exchequer] “and this
kind of hammered money continued through all the reigns of succeeding
Kings and Queens till about the year of our Lord 1663, when by several
warrants and command of the King, Charles the Second: to wit, by one
warrant, dated the fifth of November, 1662; one warrant, dated the
eighth of April, 1663; and a third warrant, dated the twenty-fourth
of December, 1663; the other sort, called _milled money_, was first
fabricated to be current in England in this manner: first, the gold or
silver is cast out of the melting-pot into long flat bars, which bars
are drawn through a mill (wrought by a horse), to produce the just
thickness of guineas, half-guineas, crowns, half-crowns, shillings,
&c. Then with forcible engines called _cutters_, which answer exactly
to the respective sizes or dimensions of the money to be made, the
round pieces are cut out from the flat bar, shaped as aforesaid (the
residue whereof, called sizel, is melted again), and then every piece
is weighed and made to agree exactly with the intended weight, and
afterwards carried to other engines (wrought secretly), which put the
letters upon the edges of the larger silver pieces, and mark the edges
of the rest with a graining. The next thing is the blanching, performed
as above; and at last every piece is brought to the press, which is
called the _mill_ (wrought of the strength of men), and there receives
the impression, which makes it perfect _milled_ money.”
The processes now used are as elaborate as the old methods were simple;
but considering the requirements of the present day, and the enormous
quantity of money produced, it must not be expected that our coins
will, for depth of engraving, bear comparison with those of the Romans,
who, though succeeding in producing finished works of art, seem to have
forgotten the wear and tear to which they would be subjected, and so
left them, as a rule, free from a protecting edge; hence they would
lose their image and superscription at a far earlier date from their
birth or manufacture than would well-made coins of the present period.
It was formerly believed that gold could be sent to the Mint to be
coined free of charge to the importer; such, however, was not the case.
By the Act 33 Victoria, cap. 10, several Acts relating to the coinage
are repealed, and all persons[7] obtain the right to send gold to the
Mint to be coined on the following terms:—
“8. Where any person brings to the Mint any gold bullion,
such bullion shall be assayed and coined, and delivered
out to such person, without any charges for such assay or
coining, or for waste in coinage. Provided that (1)—If
the fineness of the whole of the bullion so brought to the
Mint is such that it cannot be brought to the standard
fineness under this Act of the coin to be coined thereout
without refining some portion of it, the Master of the Mint
may refuse to receive, assay, or coin such bullion. (2)
Where the bullion so brought to the Mint is finer than the
standard fineness under this Act of the coin to be coined
thereout, there shall be delivered to the person bringing
the same such additional amount of coin as is proportionate
to such superior fineness. No undue preference shall be
shown to any person under this section, and every person
shall have priority according to the time at which he
brought such bullion to the Mint.”
The standard for gold is fixed by the new Act at “Twenty-two carats
fine and two carats of alloy in the pound weight troy”—the same that
was specified in the 3rd Edward VI., 35th Elizabeth, 2nd Charles I.,
and 18th Charles II. Silver is maintained at the former standard of
“Eleven ounces two pennyweights fine silver and eighteen pennyweights
of alloy in every pound weight troy.” Until the passing of this Act
silver was coined under that of George III., which repealed the Act 18
Charles II., as regards the coining of silver free of charge. The Act
33 Victoria, cap. 10, repeals that of George III., but fails to make
provision for the coining of silver, which is therefore now coined
under the Common Law; yet the new Act specifies the weight and fineness
of the silver coinage. The omission was made because the Chancellor
of the Exchequer thought it “unfair to introduce silver to this Act
as it is a source of revenue;” a little later I will examine this
statement.[8]
The Bank of England is practically the only “importer” of bullion to
the Mint, and by coinage makes a considerable profit merely from its
exceptional circumstances. By its charter and by Act of Parliament
it is compelled to keep a stock of bullion equivalent to the excess
of its authorised issue of notes—such authorised issue being secured
by “Government debt” and “other securities”—which at the present
time is fifteen millions; and gold, when at the Mint for coining, is
esteemed as being still at the Bank. By the Act 7 and 8 Victoria, cap.
32, section 4, the Bank of England is compelled to purchase bullion,
previously melted and assayed at the cost of the seller, at the rate
of £3 17_s._ 9_d._ per ounce of standard gold, paying for it in Bank
of England notes. Assuming that all the gold thus purchased is coined,
the Bank makes a profit[9] of about £2,000 on each million. When its
authorities desire to coin gold they give notice at the Mint, and
subsequently send at stated intervals “importations” of say 200 ingots
of gold, each weighing about 180 ounces, and previously assayed. Upon
the arrival of these ingots at the Mint, they are taken to an office,
where, in the presence of an officer from the Bank of England, a
small piece is cut from each ingot, and hammered out into a kind of
strip. This piece is then put into a paper marked with a letter which
corresponds with the mark or letter on the individual ingot from which
it was taken. This having been effected for each ingot, the pieces are
forwarded with their respective ingots to the Mint Office, where their
weight is determined and compared with that charged by the Bank of
England. The pieces which have been hammered out and placed in a marked
packet are called the “assay pieces.” The assay pieces are sent to the
resident assayer in the Mint, who estimates and reports to the Master
the amount of pure gold in each ingot. The report of the resident
assayer is then submitted to the Bank authorities, and if they find it
to agree with their own assayer’s report, the ingots are retained for
operations in the Mint. When it is desired to get the ingots of gold
into a form fit for coining, they have to be alloyed with copper, or
fine gold must be added, so as to bring them to standard or crown gold,
which consists of 22 parts of pure gold and 2 parts of alloy, or 91·66
per cent. of gold and 8·33 per cent. of copper in 100 parts. Copper is
usually employed because it is cheaper, and forms a harder alloy than
silver.
[Footnote 7: See page 169.]
[Footnote 8: See pages 126, 144-156.]
[Footnote 9: See pages 126-127, 168.]
Supposing there are 100 ingots, having a total weight of 18,000 oz.,
and by assay it has been found that they contain 17,900 oz. of pure
gold, it is required to bring them to the standard fixed by law. A
rule-of-three sum tells how much alloy or how much gold is to be added.
So, if 22 parts of pure gold require 2 parts of alloy, how much alloy
will 17,900 parts require? The fourth term of the following proportion,
viz., as 22:2::17,900:1,627·027, will show how much is to be added; but
since there are already 100 oz. of alloy present, as indicated by the
fact that 18,000 oz. contain within themselves only 17,900 oz. of pure
gold, it is only necessary to add the excess required, viz., 1,527·027,
so that these 100 ingots will produce 19,527·027 oz. of standard gold.
Had the ingots been found to contain more alloy than is required,
it would have been necessary to add so much pure gold as would have
rendered the whole standard. The proportions of the metals having been
determined, the whole mass is divided so as to make about 1,200 oz.
of gold and alloy for each melting-pot. In practice it is customary
to take the estimated amount of gold in a given number of ingots, and
add so much alloy, or so much pure gold, as shall bring those ingots
to standard, the whole weight being generally about 1,200 oz.; this is
called _potting_ the ingots. Ingots are almost invariably melted, and
cast into bars for sovereigns.
I must here mention that the various illustrations I have introduced
were originally used for the article “COINING” in TOMLINSON’S
“CYCLOPÆDIA,” and the permission to use them here has been generously
granted to me by _Messrs. Virtue and Co._, whose property they are.
In the illustrative engravings, the initial letters used to indicate
the different parts are made to take their places in accordance with
the order in which the various parts of the machine under description
come into play, so that by tracing out the alphabet in any figure, the
reader will see the consecutive action of the parts of the machine he
is studying.
[Illustration: Fig. 1.—Gold Melting.]
Fig. 1 represents the arrangements for melting the ingots with their
alloy, for producing standard gold. In the Mint there are seven
furnaces: each furnace, A, is 12 inches square and 24 inches deep to
the top of the bars, which are seen at the ash-pit B. The pot C is
made of a mixture of Stourbridge clay and plumbago, hence called a
_plumbago pot_; it is 9¼ inches deep, and 7 inches across at the top
inside. The pot, previously annealed, is placed in the furnace on a
_bottom_ which stands upon the two centre bars. The bottom is intended
to shelter the base of the pot C from the stream of air which is
necessary to the combustion of the fuel, but which would damage the
pot. The pot is then covered by its muffle and lid, and surrounded by
fuel, which, as it burns up, warms and then heats the pot to redness,
but so gradually that there is no great risk of breaking the pot. When
the pot has become of a full red heat, the ingots are carefully placed
in it, and the alloy is added by means of the funnel I: the pot is
then covered up, and allowed to remain till the whole mass of metal
has liquefied. The foreman then stirs it with a rod made of the same
substance as the pot, and allows it to remain till the fluid mass has
reached a peculiar temperature, known by experience as that at which
the metal, when poured into a mould, forms the most solid and workable
bar. This temperature having been gained, the two outside bars at B
are removed, the ash-pit is then covered to protect the men’s feet,
and the firing poked out. The lid and muffle are next removed from
the pot, and the pot lifted by an assistant from the furnace by the
crane D. The foreman then conveys the pot C, by means of a pair of
tongs which clasp it, to the frame of moulds, when an assistant brings
forward a loop of iron, suspended by a chain and cord from the roof
of the building, and passing the loop of iron over a button on the
end of the lower clamp of the tongs, as shown at E, F, supports the
weight of the pot by the cord, as indicated at G. Previously to the
melting, pieces of charcoal are placed at the bottom of the pot for
the purpose of reducing any oxide that may be present in the alloy—and
Dr. Percy has found that copper can dissolve 13·50 per cent. of oxide
of copper—because oxide of copper, when dissolved in standard gold,
frequently renders the mass so brittle that when the bars produced are
passed between the rollers they crack and break, just as does gold
containing minute quantities of lead or zinc. The influence of oxide
of copper on standard gold was thus very marked in 1859, when a large
proportion of the gold was so brittle, that if a bar were dropped on
the floor, or tapped with a hammer, it broke, just as heated brass
breaks under similar circumstances. Mr. Richard Smith had some years
since pointed out that if copper in which oxide of copper is dissolved
be poured through an atmosphere of coal gas, all the oxide is reduced.
I therefore submitted this gold to the process thus suggested to reduce
all the oxide of copper, and produced bars so tough that they could
not be broken by a sledge hammer unless after repeated bending by that
means. Yet this gold was not thus cured of its brittleness, but was
treated peculiarly, as will be seen in a future place.[10]
[Footnote 10: See pages 50-53.]
When the metal is fused, the charcoal which was placed at the bottom
is brought to the surface by stirring, and as it rises through the
fluid alloy, reduces the oxide of copper, and remains on the surface to
protect the alloy from the action of atmospheric oxygen. In order to
prevent it from falling into the moulds, the assistant holds a piece
of stick at the mouth of the pot, thus allowing the gold to pass, but
stopping the charcoal. The foreman, in the case of gold, judges almost
wholly by the eye, but in the case of silver by the ear, as to when
the moulds are filled. The metal poured from each pot forms four bars.
The moulds H are made of iron, cast into such a form that each piece
viewed from the top has the form of the letter =T=, so that three
pieces placed together form two moulds; the whole of the set is held in
its position by cross-bars, L, which fit into notches cut in the main
frame M, where will be seen two powerful screws by which the moulds are
forced tightly together after the cross-bars L are fixed. J represents
the pots placed so as to be kept dry and ready for use; K, the wheels
and tram on which the frame of moulds runs. The whole of the set of
moulds having been filled, the screws at M are loosened, the bars, L,
removed, and the parts of the several moulds removed, so that the bar
in each mould is exposed to view. The workman takes each bar as it is
exposed by a pair of tongs, and plunges it into a cistern of cold water
to insure rapid cooling, and then places it on a bench, where the
bars produced from each pot are separated and marked with a number, to
indicate the pot from which they were poured, and the entire set with
letters, to indicate the day on which the melting took place. After
these distinctive marks have been placed on the bars, two assay pieces
are taken from the bars from each pot.
[Illustration: Fig. 2.—Silver Melting.]
As silver melting,[11] when discreetly conducted, is slightly different
in some of its details, it will be well to describe it here. In Fig. 2,
A indicates the furnace with the front removed, to exhibit the internal
arrangements. The furnace is circular, and is 21·5 inches across, and
31 inches deep. The bars, which are represented by dotted lines, are
removable at will. The _bottom_ B stands on the centre bars, just
as in the case of gold melting: it is filled with coke dust, which
retains any silver issuing from a small accidental crack or pin-hole
in the pot, and also offers a non-conducting medium for the pot C to
rest upon, it being necessary to avoid the abstraction of heat by the
current of air against the base of the pot. A muffle, D, is placed on
the pot, and upon this muffle the lid E rests. The pot is circular,
and provided with a lip, to facilitate the pouring of the metal; it
is made of wrought-iron, 12 inches across at the top, and 15 inches
deep, and when melting for florins is charged with 4,800 ounces of
silver. As in the case of gold, so with silver, the metal is alloyed
with copper; standard silver being composed of 222 parts of pure silver
and 18 parts of copper in 240 parts, or 92·50 parts of silver and 7·50
of copper in 100 parts.[12] The calculations based on the assays from
ingots are just the same as in the case of gold. The ingots are put
into the pot, and the lid is placed on the muffle (which is intended to
prevent metal from falling over the top of the pot during the process
of fusion, as sometimes might happen when _scissel_[13] is melted),
and the furnace is then closed, so that the air enters through the
bars, and passes into the chimney through the flue F. The lid of the
furnace G is provided with peep-holes, by which the temperature can
be regulated at will, while they also admit of a survey of the state
of the furnace. When the fusion is complete, and carried so far as
to raise the fluid metal to the necessary temperature, the bars of
the furnace, with the exception of those which support the pot, are
removed, and the fuel is poked out, because the pot at this temperature
is so soft that it would be _torn_ if it were pulled through the fuel.
The lid and muffle are next taken off by tongs, and the crane is swung
round by the handle, H, till its tongs are brought over the furnace,
when, by working the handle I, the tongs J are lowered till they come
to the pot; the foreman then makes them seize the pot, and by a signal
gives his order for the raising of the pot from the furnace. Pieces
of fuel and iron scaling are knocked off from the pot by the foreman
with a brush kept in a crucible of water, indicated by V at the foot
of the crane. The crane is then swung round by H, till the pot is over
the cradle K, when it is lowered and secured in the cradle by the
screw, shown at C. The frame of moulds is now run under the lip of the
pot, and the foreman, by means of the handle L, which will be seen to
communicate with the wheels M, and the rack N, tilts the pot so that
the fluid metal may pour in a good stream into one of the moulds O,
until, by the sound, he judges it to be full; he then lowers the pot,
while his assistant, who is also watching the filling of the moulds,
turns the handle P, which, by the wheel Q fitting into the rack R,
moves forward the frame of moulds so far as to allow another mould to
come beneath the lip of the pot, to be filled as before. The fluid
silver in the melting-pot is covered with charcoal, for the same reason
as explained in gold melting, and this is kept back by means of a large
piece of charcoal laid at the mouth of the melting-pot. The frame of
moulds runs on wheels S, and at T is provided with a rack and pinion,
by which the moulds may be moved farther from or nearer to the lip of
the pot, which, as it is tilted, is continually altering its relative
position to the mouth of the moulds, and would, were it not for this
arrangement, pour its metal outside of, or upon the moulds, instead
of into them. The moulds are formed of =T= pieces, in the same manner
as the moulds for gold, and are secured in their position by the same
method, the cross-bars being shown at U. The bars, having been taken
from the moulds, are cooled in water, and distinctively marked, as in
the case of gold. Assay pieces are cut from them, but in the case of
silver three assays are taken from the bars produced from each pot.
[Footnote 11: See pages 129-138.]
[Footnote 12: See pages 3, 73.]
[Footnote 13: This word is explained at page 35.]
The bars for different denominations of coins are proportioned in their
width, so as to admit of two rows of blanks being cut from the fillets
produced from them. The following statement gives the whole facts
concerning bars for each coin, as used in the Royal Mint. It would be
well to produce bars of a uniform thickness of 0·50 inch, as such bars
may be cast solid, and when cast produce better fillets with half the
rolling, without the cost of annealing. There would be also another
advantage, for the blanks obtained from the fillets produced from bars
0·50 inch thick would not require annealing, and would thus save the
cost of that process, as well as the loss occasioned by it, while the
coins produced would wear immeasurably longer in circulation. There are
other considerations why this thickness should be at once adopted, as
will be shown when the subject of loss by coining is explained.
I am glad to notice that Mr. Fremantle, in his Report on European
Mints, proposes to adopt my recommendation, as shown by the following
passage, page 9:—
“... It would seem to be a question whether in a newly
organised Mint considerable time and labour might not be
saved by reducing the size of the moulds in which both gold
and silver bars are cast. The result would be that, as
bars would be thinner when first subjected to the process
of rolling, the time now occupied by that process would
be sensibly diminished. It should also be mentioned that
although there is great difficulty in producing sound
castings if the thickness of the bars should be reduced, it
might nevertheless, for the metallurgical reasons which Mr.
Roberts points out, be advisable to make this alteration.”
There is really no “_difficulty_ in producing sound castings if the
thickness should be reduced;” but I fear there are many DIFFICULTIES
in the Royal Mint itself. Indeed the casting of the bronze bars—whose
thickness is less than that I propose for those of gold—gives evidence
of the ease with which thinner bars may be produced; yet against
_these, insuperable difficulties_ were urged until I experimentally
demonstrated how easily they could be cast.
STATEMENT OF PARTICULARS AS REGARDS BARS USED FOR COINING.
+--------+---------------+-------+--------+----------+--------+
| Metal. |Denomination of|Length.|Breadth.|Thickness.|Average |
| |intended coin. | | | |Weight. |
+--------+---------------+-------+--------+----------+--------+
| | |Inches.|Inches. | Inches. |Troy oz.|
|Gold | Sovereign | 24 | 1·375 | 1·000 | 320 |
| | Half-Sovereign| 24 | 1·125 | 1·000 | 250 |
+--------+-----------------------+--------+----------+--------+
| | Crown | 22 | 2·750 | 1·000 | 300 |
| | Half-Crown | 22 | 2·500 | 1·000 | 240 |
| | Florin | 21 | 2·125 | 1·000 | 220 |
|Silver | Shilling | 21 | 1·437 | 1·000 | 150 |
| | Sixpence | 21 | 1·125 | 1·000 | 120 |
| | Fourpence | 21 | 0·875 | 1·000 | 96 |
| | Threepence | 21 | 0·875 | 1·000 | 96 |
+--------+-----------------------+--------+----------+--------+
| | Penny | 24 | 2·500 | 0·375 | 100 |
|Bronze | Halfpenny | 24 | 3·000 | 0·375 | 117 |
| | Farthing | 24 | 3·000 | 0·375 | 117 |
+--------+---------------+-------+--------+----------+--------+
It is to be regretted that crowns, half-crowns, and fourpences are no
longer coined. It has been represented to me by many manufacturers and
others who employ vast numbers of men, that the disuse of the fourpenny
piece has caused considerable inconvenience in the weekly payments to
their workpeople. The objection to this coin would appear to be that it
is so nearly the diameter of the threepenny piece; but this is obviated
by the fact that the edge of the latter is plain, while that of the
fourpenny is crenated or “milled.”
The assay pieces,[14] when cut from the bars, are placed in the
divisions of a tray going from left to right, so that there can be
no mistake as to the number of the pot from which the metal comes;
each assay piece is then placed in a small envelope, marked with a
distinctive mark, to characterise the pot from which it came. The assay
pieces are sent in equal numbers to the two non-resident assayers,
who determine, irrespectively of each other, the amount of gold found
in each piece. Suppose we trace one assay piece, and imagine that 120
are undergoing the same process at the same time. The assay piece is
flattened out into a kind of ribbon, and from it three pieces are cut,
each weighing half a gramme. Each piece of this weight takes the name
of a _thousand_, and is represented by the figures 1,000; but of course
it may be called a pound, a ton, or by any other denomination. Each
piece is wrapped in paper, with three times its weight of silver in two
pieces, both metals being of the same thickness. The parcels, as they
may now be called, are ready for the next process, and are arranged
in their proper places from left to right in the divisions of a tray,
and taken to the assaying furnace. In the assaying furnace is placed a
Payen[15] muffle, or kind of oven, perforated at places so as to allow
a limited amount of atmospheric air to pass from the interior through
its sides into the furnace. The muffle is surrounded with fuel, so that
it is kept at a good—almost white—heat. On the floor of the muffle is
sprinkled some bone ash—obtained by burning bones to whiteness—and on
this bone ash is placed a set of 40 cupels, or little cups, made of
compressed bone ash, and about as big as a florin, and so deep as to
hold about half a teaspoonful of water. When the cupels have been in
the muffle long enough to become red hot, a piece of lead of about nine
times the weight of the gold to be assayed is put into each cupel,
taking care not to let any lead fall over, or it would destroy the
muffle. So soon as the lead has melted, the paper parcels containing
the gold and the silver are placed one in each cupel of melted lead.
In a short time the gold and silver melt together, and, as it were,
dissolve in the lead; then a kind of circulation of the fluid metallic
mixture is observed to take place; and during this circulation, the
lead, as it is presented to the surface, meets with the oxygen of the
atmosphere, and combining with it, forms oxide of lead, which at that
temperature is fluid, and drains into the substance of the cupel,
carrying with it the copper and other impurities contained originally
in the gold, leaving in the cupel a button which contains all the pure
gold and the silver. The cupellation occupies about ten minutes, and
at the end of that time the little mass of fused metal is observed to
brighten up, the signal by which the assayer knows that the process is
finished, and he withdraws the cupels one by one, tilting the fluid
globule on one side, that it may incorporate with it any small globule
which may chance to be upon the side of the cupel. Some assayers
close the doorway of their muffles as the time of the brightening up
of the assay approaches, to avoid the access of the atmosphere till
the buttons have become solid, because the button of metal—by its
silver—absorbs oxygen; and giving off this oxygen at the moment of
solidification, spurts or opens, leaving the button hollow or ragged.
This precaution is not thought necessary by all assayers, nor, indeed,
is this system invariably followed, for some prefer to wrap the gold
and silver in the lead foil which is to be used, and do not care to
have the precious metals of identical thickness; these assayers use a
smaller proportion of silver, viz., 15 parts to 6 of standard gold,
or 17·50 to that which they judge to be _fine_, with a view to avoid
the danger of “spurting;” they also save time by withdrawing the whole
batch of cupels on a tray by means of a peel. The button is taken from
the cupel as soon as it has been detached, either by dropping a little
water on to it, or by allowing it to cool spontaneously, and it is
then hammered out into a strip and annealed. It is next rolled into
a ribbon or fillet, and again annealed, after which it is curled up
into the form of a letter S. Some prefer to roll the piece into a kind
of cushion, but in such a case it is more difficult to remove all the
silver; the proper plan is to expose as large a surface as possible to
the action of the acid in the next operation.
[Footnote 14: See pages 9, 53.]
[Footnote 15: That is, made by Payen, of Paris.]
The S-shaped fillet is put into a flask of nitric acid of specific
gravity 1·23, and the flask is placed in a little cup of brass,
which stands over a small gas-burner, while the neck of the flask
enters a kind of flue, through which a current of air is continually
passing into the chimney of the furnace. The flask being placed in
its position, the gas is lighted, and a gentle heat applied, when the
nitric acid dissolves out the silver from the S-shaped fillet, and is
known to have done its work when red fumes cease to be evolved. The
acid is then poured off, and the remaining sponge of metal is washed
with distilled water, and boiled with concentrated nitric acid, which
removes the remainder of the silver. The sponge of gold is now washed
with water, to remove the nitrate of silver, and is then heated to
redness in a capsule to render it tough, for in its spongy state it is
so rotten that it will not bear to be touched; and although it remains
spongy, it is toughened by being heated to redness. It is now called
a _cornet_. This spongy state is a consequence of the addition of
silver, the presence of which, and its subsequent removal, produce a
separation of the particles of the gold. The gold is thus formed into
a kind of network or sponge, so that the acid can get at every part of
it, and remove any metal which is soluble in the acid. Diluted acid
is used first, because if there be any lead left it is dissolved out,
and because the action of the strong acid is so violent, that part of
it would probably be carried out from the flask. Nitric acid, when
boiling, is liable to form bubbles of gas, which expanding, give rise
to what is called _bumping_; hence it is usual to put a charred pea
into the flask, and this, floating on the surface, causes a more even
flow of vapour and gases, and so prevents bumping. It is probable that
the charred pea determines the boiling at one particular temperature,
for it is found that water, if it be floated in a fluid of a higher
boiling point than itself, may be raised considerably above its
ordinary boiling point, although remaining quiescent till disturbed
by a rod or point. The cornet is next weighed, and as it has been
begun under the idea that it was a _thousand_—1,000—all that it weighs
short of 1,000 is the alloy which has been removed, the object having
been to determine how much pure gold was present in the alloy. There
is, however, a source of error in the process which requires to be
explained.
It is found to be practically impossible to remove every trace of
silver from the cornet; it is therefore necessary to make an allowance,
the amount of which is determined by a _proof_. The proof consists of
a mixture of gold and silver of known proportions, so that if all the
silver be removed from a thousand—1,000—the remaining cornet should
weigh exactly 916·6. Four of these proofs are worked with each batch of
assays—a batch being 120 assays—under precisely similar circumstances,
every precaution being taken that the four shall be equally distributed
over different parts of the furnace, &c. Now suppose that the proofs,
instead of weighing 916·6, as they would weigh if the whole of the
silver were removed, were found each to weigh 916·9; it would be known
that 000·3 of silver had been retained, and must be deducted from each
of the whole batch of assays. If the assays of coins exceed the limits
of from 917·6 to 915·6, they are repeated, as it is assumed that an
error has arisen. The convenience of considering the ½ gramme as 1,000
consists in the fact that 1,000 parts of standard gold contain 916·67
of gold and 83·33 of alloy; so that the result having been arrived at
without any calculation, one source of error is avoided and time is
saved.
Messrs. Johnson, Matthey, and Co. have invented a tray of platinum
capsules or thimbles, into which the assay pieces are placed for
treatment with acid, instead of into the ordinary glass vessels over
gas-burners. The advantages of this invention are too manifest to
require elaboration; but saving of acid, gas, labour, and risk of
error are amongst the chief of them; and besides, the plan has been in
successful operation in their own assay offices in Hatton Garden, as
well as in other important assay offices, for several years past. The
first cost would seem to be the principal objection to this plan of
Messrs. Johnson, Matthey, and Co.; but this is really a small matter,
for the apparatus becomes stock in trade, and its cost should be
viewed simply as so much capital, whose interest is paid by the saving
effected in glass, but more especially by the smaller amount of acid
actually employed, while the platinum can at all times be sold for
nearly its original cost as old metal.
The mode of operation is as follows:—A stand of slate is so arranged
that a means of heating is made to rest on its base. For this purpose
a jet of gas is preferred; where, however, gas cannot be obtained,
an ordinary oil lamp or a charcoal fire may be used. On a shelf over
the source of heat are placed two or three receptacles of platinum,
each communicating with a vessel made of porcelain, provided with
three necks and an overflow pipe. There is a kind of sieve or tray of
platinum, so arranged as to carry from 16 to 100 thimbles of platinum,
and provided with a handle, so that this tray, with its charge, can be
manipulated at pleasure. The thimbles vary in size according to taste,
but each one is cut or slit at the bottom, so that the solution of
silver as it is formed may by its density fall out, and allow the clean
acid to take its place.
When an operation is to be performed, the tray filled with the charged
thimbles—that is, containing the assay pieces—is placed in one of the
platinum receptacles or boilers, and heated to a fitting temperature;
when the desired effect is produced, the tray is lifted into another
receptacle, and again heated; this may be carried to three times if
necessary. The products of decomposition of the acid go, with the acid
which evaporates, into the porcelain vessel, where the free acid falls
through the overflow pipe into a proper chamber, while the acid fumes
pass into the flue through the third neck before spoken of. The parted
assays having been washed by several immersions in boiling distilled
water, without removal from their thimbles, have now to be dried and
annealed in a platinum muffle, so formed as to fit into an ordinary
muffle, and, after annealing, to be weighed in the usual manner, having
saved at least 75 per cent. of the usual trouble.
It is almost needless to add that the system of _proofs_ above
described must be also used with this process.
The assay for silver is not so tedious, as it is finished at the point
where it leaves the muffle on the cupel; but up to this point it passes
through precisely the same process as the gold.
It will have been observed that the event of the process of assaying is
to exhibit the proportion of _bullion_ which may be present in a given
weight of mixed metals, but that it does not demonstrate the character
of the substance which forms the alloy, because this is assumed to
be copper or silver. In practice it is found that the alloy may be
a mixture of copper or silver with lead, mercury, antimony, arsenic,
tin, or zinc, in varying proportions, but whose sum does not exceed the
rate per centum in relation to the bullion which is allowed by law. The
existence of minute proportions of lead, mercury, antimony, arsenic,
tin, or zinc is a matter of great concern, for these, when present, add
indefinitely to the difficulties of the coining departments.
Under the present system, complete analyses of bullion imported for
coining are a practical impossibility. I would therefore propose to
abolish the office of non-resident assayer, and then to appoint two
resident assayers, who should conduct their operations in independent
laboratories—already existent—and a condition of whose appointment
should be an agreement to conduct, when so directed by the Master
of the Mint, complete analyses of the bullion submitted for assay.
The information thus obtained would enable the melter, by processes
subsequently explained,[16] to remove all those substances which
are _now_ found to be fatal to the coining of certain bullion. The
appointment of officers possessing such ability would be an equal
guarantee with the present for the faithful preservation of the
integrity of the coinage. This suggestion has been adopted and
recommended—so far as regards the resident assayers—by Messrs. C. W.
Fremantle and C. Rivers Wilson, in their “Reports on the Mint,” 1870.
Indeed two assistant assayers have been recently appointed.
When the assay reports arrive, the Master determines whether the metal
has been found within the limits, and if he be satisfied he writes on
the assay reports “Passed,” and signs the reports. The Deputy-Master
retains the reports as his warrant, and then issues his order for the
delivery of the bars by the melter to the rolling room, as recommended
in my report dated 29th January, 1859; but, as the accounts are kept by
weight, every set of bars is weighed by the officer who receives them
into that room before he gives them to his men to work into fillets.
When, in 1856, I took charge of some departments in the Royal Mint,
I found that the system of weighing was extremely loose. Officers
were plainly told that if they ventured to satisfy themselves as to
the weight of bullion they had received—in fact, to determine whether
they received what was charged to them—“they would be paid out.” This
state of things led men to accept _any_ weight. But I objected and
resisted; for I found that the average on each day’s work as received
amounted to an habitual minus of five ounces on the weight charged
on silver, while on gold it was seldom so little as one ounce. In
illustration I will state one case which occurred. I delivered 7920·00
ounces of gold to the Mint Office. When that gold was received,
the official weigher gave me credit for 7918·15 ounces, which was
a deduction of no less than 1·85 ounces. I appealed to the Master,
who by written order directed the gold, the weight of which was thus
disputed, to be weighed by Mr. Pilcher, the officer of the weighing
room, in the presence of witnesses whom the Master nominated. Mr.
Pilcher complied with this order, and gave a certificate, signed by
the deputed witnesses, in which he stated that the gold under dispute
weighed 7919·98 ounces—that is, that it differed in weight as charged
by me to the Mint Office 9·60 grains instead of 888·00 grains, the
difference which the official weigher had deducted from the bullion
I had delivered to him. The custom had been to weigh silver to 0·50
ounce, and gold to a pennyweight; but I introduced the system of
weighing silver to 0·10 ounce, and gold to 0·01 ounce, and at the same
time induced the Master to order new balances of superior construction
for the coining department, and one specially devised by Mr. James M.
Napier for use in the Mint Office. Of this balance, received after
having been ordered for some years, it will be sufficient to say that
it appears to be extremely accurate when properly used, and is then
capable of great results; but, unfortunately, the system is such that
those who are admittedly unfit may be promoted to important posts, just
because they are senior, and not because of superior fitness for the
work. This fine balance, therefore, becomes equal to a good rifle in
the hands of a bad marksman. Great accuracy having been enforced, the
weighing is now improved, but is still far from perfect, because the
officers are compelled to abide by the decision of the weigher at the
Mint Office, who, as beforesaid, may be unfit for his office, while
the officers themselves are debarred from all checks, by the removal
from the coining department of the set of standard weights, which were
bought on purpose that those gentlemen might check their own weights as
to accuracy. The Master’s order for the removal of these weights was in
the following terms:—
[Footnote 16: See pages 81-82.]
“The standard weights hitherto kept in the weighing room
are permanently transferred to the Mint Office. A new set
of standard weights to be made for the Mint Office. The
coining department weights to be examined by Mr. ——
——, and compared with those in the Mint Office (after
these have been corrected), and reported on by him. Such
examinations to be repeated every six weeks.”
It should be observed that this order was preceded by one written on
the 2nd February, 1865, which directed that the Mint Office weigher
should be the final judge, but that any officer might demand the
re-weighing of any bullion, while the second weighing was to be final.
All appeals to pass through Mr. John Graham, the order proceeding to
direct that—
“The final decision is not to be called in question by any
other officer of the coining department.”
The latter determination, I was informed, was intended to apply to me
personally. Its immediate effect was a deduction of 0·25 ounce from the
first gold I delivered, and a consequent alteration of my book to that
extent by Mr. John Graham, who made a note in writing as follows:—
“This difference (error) may be accounted for by the
acknowledged error of three grains heavy of the Mint Office
500 oz. weight. See Œrtling’s Report.
(Signed) “J. G.”
Such being the circumstances, I submitted; but the result could be in
one direction only, for it had long been maintained that the reported
losses were but “an hallucination,” and were, in fact, a “mere
difference of weighing.”
It is true that the weights are periodically adjusted, but there is
adjusting and adjusting. These facts have been dwelt upon because
they have a most important bearing on the subject of loss and gain by
coining, to be afterwards treated of.
Between 1856 and 1866 the old scales were removed, to make room for
the superior balances of Messrs. De Grave, Short, and Fanner, the
eminent scale-makers of St. Martin’s-le-Grand, of whose balances it
is impossible to speak too highly, and of whom it is but fair to
state that the Prize Medal was awarded to them at the International
Exhibition, 1862, for their superior workmanship in balances.
Since it is necessary for the officer in charge of any department to
ascertain the exact amount he gives to his workmen, and to satisfy
the Master that they have returned—to within the limit of the weight
of one blank of whatever denomination of coin he may be working—the
bullion which they received, it became imperative to select the best
balance; and in practice that made by Mr. S. R. Short, of the firm
above named, was found to be the most serviceable. Mr. Short has
introduced minor improvements from time to time, as experience has
dictated, but the balance about to be described, after years of wear,
determines to within one grain when charged with 1,200 ounces troy. The
mode of proving the accuracy of a balance is to weigh as usual, and
having arrived at a just determination of the weight of the matter to
be weighed, to change the weights to the pan in which the matter has
been weighed, and to place the matter in the pan previously occupied by
the weights, so that both are now made dependent from the reverse ends
of the beam; if the results be identical with the former results there
can be no doubt as to the accuracy of the beam; should there be any
variation, the balance must be adjusted by minute alterations of the
knife-edges at its ends.
Mr. Napier has made his balance after the principle of Mr. Cotton’s
balance, so that it requires no adjusting screws, but I have no
personal experience of the benefits of this omission.
[Illustration: IMPROVED BALANCE (TO WEIGH 2000 OUNCES.)
BY Mʳ. S. R. SHORT, JUNʳ.]
The balance used in the rolling room of the Royal Mint is specially
adapted for the purpose. Such a balance, as already noticed, must be
accurate, as must also all the balances used in the Mint; but this
balance requires an arrangement by which the pans can be released
from the beam and held firmly while being loaded. Mr. S. R. Short has
been peculiarly happy in effecting this object, as will be seen by
reference to the steel engraving, which exhibits a fine illustration
of Mr. Short’s balance. The raising of the handle A causes the partial
revolution of the cam B—represented by dotted lines—and this, as it
diminishes, releases the lever C, which, by the rods D acting on the
point E, permits the approach of the joints on the rods F towards the
centre. The rods F work on a centre fixed beneath the table on which
the balance stands, so that the closing of their one end causes the
opening of the other. Thus the claws G recede from the wedges H, upon
which they had been fastened, and so release the pan, for the claws act
simply as a man’s hand would act in fixing the pan while it is being
loaded. Immediately upon the opening of the claws another action takes
place by the continued movement of the handle A, which causes the cam
I to rotate upon the friction roller J, affixed to a lever proceeding
from the shaft K, which at L is cut with eccentric bearings, so that
by the partial revolution of K, caused by the pressure of I upon J,
the series of supports M sink downwards from the pans N, thus obliging
the pans, with the rods which support them, to be suspended from the
supports S, which rest on the frame R. So soon as the pans are thus
suspended, the continued motion of the handle A causes the cam O to
permit the falling of the lever P, which at Q supports upon a friction
roller the iron framework R. This framework terminates upwards at the
points near S in sugar-loaf cones of gun-metal, which are intended
to relieve the knife-edges of the beam from the pressure of their
planes while the beam T is out of use, or while it is being loaded,
for at these times the knife-edges would become seriously damaged.
By the lowering of the frame R the centre knife-edge U is permitted
to rest on its plane of steel _c_, which is beautifully bedded on an
arch of gun-metal, as will be seen if the enlarged representation of
this part, and which is shown to the right, be examined. In fact, the
steel plane _c_ is secured by wedges exactly shaped to it, but for the
sake of illustration these wedges have been replaced in the enlarged
portion of the engraving by upright pillars shown against _c_, with
screws travelling through them, and intended to fix _c_ rigidly in a
given position. At the same instant that U comes into rest upon _c_,
the knife-edges V at the ends of the beam T receive the planes W, so
that the beam has now to support the weight of the matter placed in
the scale-pans, and at this time is determined the actual weight of
whatever that matter may be. The weigher, by an indicator suspended
from the beam at X, reads the oscillations of the beam on an ivory
plate at Y. At the time of weighing, the beam with its dependents
is carried by the four-legged frame of iron _b_. The frame R passes
through friction rollers of brass at _d_, which rollers maintain it in
its relative position to the beam. The weighing having been determined,
the handle A is reversed, and the beam is placed at rest; but the
vibration of the machinery in the rolling room causes a continuous
chatter of the knife-edges V against the planes W, therefore at each
end of the beam a small screw Z is made just to touch the lower edge of
the beam when it is at rest. Final adjustments which are very minute
may be arranged by _f_; while the box _e_ on the pan against G is
intended to receive small pieces of lead, which are used to compensate
for the loss by the wearing of the pans. The shaft K is supported from
the table by _a_. The beam of the balance represented in the steel
engraving measures 48·00 inches from knife-edge to knife-edge; that
is to say, it measures 24·00 inches from the centre knife-edge to the
knife-edge at either end. Mr. S. R. Short has made for the rolling
room another balance for weighing silver, and as it differs in some
important details, it is deemed wise to demonstrate those alterations
in Fig. 3, where the supporting frame R will be seen to carry three
upright pillars S¹, S², S³. The pillars S¹ and S³ are represented as
being placed on the farther side of the beam, which at those parts
is broken away, that the pieces of steel against which the pillars
are made to touch may be seen. S² touches against one of these pieces
of steel near the centre knife-edge U, and in front of the beam. The
pillar S² terminates in a point, which passes into an inverted cone,
while the point of S³ is made to pass into an inverted =V=, so that
when the beam is raised by these pillars from its centre knife-edge, S²
obliges it to take a specific position with regard to its distance from
the centre of the plane on which its centre knife-edge rests, and S³
causes it to take a perfectly parallel line. S¹ is simply a plane which
rises against a plane and steadies the other end of the beam, which by
this arrangement stands as on a tripod, and is, therefore, prevented
from moving, and in addition has its knife-edge invariably placed upon
the same part of the plane at each time of weighing, while the frame R,
by its continued lowering, drops the planes with equal accuracy on the
end knife-edges V.
[Illustration: Fig 3.—Short’s Plan for Levelling a Beam.]
[Illustration: Fig. 4.—Breaking-down Mill.]
The sovereign bars having been weighed by the officer, and given by
him to his men, are wrought in sets of twenty; each set is called
a _batch_, and each bar in the batch undergoes precisely the same
process. The bar is passed into the opening A of the breaking-down
mill Fig. 4, where it receives a considerable compression, for the
rollers B, seizing its end, drag it forward, while they roll back and
retard the progress of that part of the bar which is not between them.
The result is that the bar is lengthened, but not widened materially,
so that length is gained at the expense of the thickness, which is
regulated by the distance between the rollers. The rollers are driven
by shafts and adjusting couplings C, which are themselves driven by the
wheels D. The distance between the rollers is determined by the action
of the lever E′, which, by the endless wheels on its axle at E fitting
into geared wheels, gives motion to powerful screws shown at F, which
terminate in cups on the upper part of the upper brasses of the rollers
B, as may be seen at G. The upper brasses are kept always against the
ends of the screws by weights which are beneath the mill, but from
which levers and rods terminate at the lower part of the upper brasses,
at about the position indicated by I, so that the upper roller has
motion either upwards or downwards at pleasure, but the motion upwards
is arrested by the powerful screws F, and this point once determined
by the reading of the scale H, is fixed by the clamp J. The thickness,
therefore, of each bar in a batch is determined within certain limits;
and when each bar in the batch has been rolled, the mill is altered,
refixed, and again the rolling goes on till each bar has passed seven
times at varying pinches through these rollers. Owing to the wear
of the moulds in which the bars are cast—and which is largely due
to the presence of minute portions of antimony in the gold—the bars
are never of uniform thickness; hence bars of every denomination are
passed through the rollers on their edge, so as to reduce them to one
uniform thickness, otherwise the fillets resulting would be ragged,
and of unequal widths, which defect would cause them to produce blanks
out of _remedy_[17] as to weight. The rollers are set face to face;
the graduated scale H is then fixed at zero; if now the rollers are
separated until there be a space of 1·00 inch between them, the scale H
will indicate 50; if, however, it be desired to read a higher figure,
part of another revolution must be performed, causing the scale to
read, say 31·50 of that revolution, when the rollers will be so far
apart that sovereign bars which pass between them will, allowing for
the expansion after compression, be found to be exactly 1·375 inches
wide.
[Footnote 17: See p. 39.]
If now these bars be rolled on their sides, the mill must be turned
down till the scale reads 45, when, if the bars be passed through, they
will measure as under for width and thickness at each successive pinch.
A _spring-pinch_ means the passing the bar once more through the mill
without altering the distance between the rollers.
A sovereign bar passed Becomes a fillet or ribbon—
through the rolling mill— Inches wide. Inches thick.
At 45·00 1·450 0·775
” 35·00 1·540 0·610
” 26·00 1·610 0·460
” 19·00 1·665 0·335
” 14·00 1·696 0·250
” 10·50 1·712 0·194
” 8·50 1·765 0·148
” 7·00 1·778 0·129
” 1st spring-pinch. 1·778 0·127
” 2nd ” ” 1·778 0·120
” 3rd ” ” 1·779 0·118
” 4th ” ” 1·781 0·117
When the bars have passed through the rollers at 10·50 they have become
of great hardness, and of considerable length, say 6 or 8 feet. They
are then taken to the shears K, where their hollow ends are cut off,
and the bars cut into lengths of 18 inches; or rather, such was the
practice when it was considered wise to obtain as much coined money as
was possible from the bars; but recently, under other considerations,
the old plan of the moneyers has been re-introduced, that of shearing
the hollow ends from the bars before rolling. In this process there
is needless waste, and it is to be hoped that the proper practice
will be reverted to, for under that system the ends averaged 4·26 per
cent., while under the re-introduced one it amounts to 7·03[18] per
cent. on the bars, and for the following reason. When the metal is
poured into the moulds, it almost immediately solidifies, and while
solidification is going on contracts in volume, leaving a kind of cup
of metal or hollow part on the top of the bar. In the act of rolling,
the bar maintains an equable width until this hollow part is reached,
when it suddenly expands, and at this point the workman shears off
the defective part of the bar, whereas in the other case he shears
off the hollow end until his eye fails to discover the effects of the
shrinkage; hence the loss of 2·77 per cent. on the produce of fillets,
as well as the loss in wages for melting the bars. The shears may be
regarded as large scissors driven by a drum on the same shaft that
carries the driving wheel for D. The drum is eccentric, so that at each
revolution the shears are caused to open and shut. The bar being placed
between the jaws K, the long end L of the shears is raised by the drum,
and the piece is cut off. The shears may be closed and the end of L
suspended, when out of use, by a hook on the end of the screw worked by
the lever M. The length at which a bar is to be cut off is regulated by
the gauge shown at N.
[Footnote 18: See page 112.]
[Illustration: Fig. 5.—Annealing Furnace.]
The sheared bars are placed in copper tubes, the tops of which are
luted on with clay. It is imperative that the copper tubes should be
made without solder, because this fuses at a temperature below that
which is required to anneal the gold; if present it would run down
upon the hot gold, and cause it to fuse and alloy with the solder,
thus spoiling the work and entailing expense upon the coiner. The
tubes which are used in the Royal Mint are made by Messrs. Benhams
and Froud, of Chandos Street, Strand, who, after considerable pains,
arrived at a method of making the tubes in such a manner as to entirely
satisfy the requirements of the Mint. The tubes A are placed on an
iron carriage B, which is then run into the furnace, as shown in Fig.
5. The door of the furnace C is closed by raising the counterpoise D;
the heat of the furnace is regulated by the damper E. The apron F is
sometimes of use in annealing very long silver bars. After remaining
in this furnace for twenty minutes, the carriage is withdrawn, and
the tubes, taken with tongs, are plunged into cold water, to cool the
gold as rapidly as possible. The rapid cooling of gold and silver
gives to each metal a peculiar character, which is of value in the
after processes, and prevents the access of the atmosphere, which, in
prolonged cooling, would cause the oxidation and consequent removal of
so much copper that the alloyed metal would become too rich in gold
for circulation as coin. The annealing of some metals is effected not
so much by the continued heat as by the slow cooling; it is therefore
wise to raise the metal to its full heat as rapidly as possible, and
then so to arrange matters that it may cool very slowly. This method
does not hold good in the case of the precious metals and of copper,
for they become, under such treatment, so soft, malleable, and pasty
as to stick to the machinery, and thus to cause considerable trouble
and loss. After annealing, the bars, which are now called _fillets_,
go again to the breaking-down mill, through which they are passed with
the scale indicating 8·50, then at 7·00, and after this are submitted
to another pinch without altering the scale at all; so that what is
called a _spring-pinch_ is given, with the intention of effecting the
reduction of the fillet to one uniform thickness, for the breaking
down and subsequent rolling cause the fillets to become much thicker
in their middle than at their sides. The spring-pinches reduce this,
while at the same time they diminish the elasticity of the metal, and
fit it for the other mills. It will be seen, by reference to the above
table, that the widening of the fillet is very trifling; but width may
be gained to any desired extent, at the will of the workman, if the
bars be submitted to a heavy pinch instead of a series of light ones.
The fillet having been submitted to the fourth spring-pinch, is gauged
on its side by a steel instrument, of which Fig. 6 is a representation.
It is a hollow wedge, which is graduated to the thousandth of an inch.
Supposing that the opening from A to B were extended until it were
one inch wide at A, the space would be divided between it and B into
1,000 parts, and then every fillet passed into this opening would stop
at a given point, say, for instance, at 140; such being the case,
every part of the same fillet should be arrested precisely at the same
point. The fillets are reduced till they measure 117 on this gauge,
and are consequently 0·117 inches thick. They are then passed to the
next mill, where they receive four light pinches, and then to a third
mill, where they receive two more very light pinches, and by means of
these six pinches are reduced in thickness to 0·075 inches. They then
pass to another mill, still finer than any of the preceding, and here
are submitted to four very light pinches, by which they are reduced to
0·058 inches, and are finally finished at the sixth or gauging mill,
where they receive three pinches, and are then 0·053 inches thick by
1·829 wide.
[Illustration: Fig. 6.—Small Gauge.]
[Illustration: Fig. 7.—Gauging Mill.]
[Illustration: Fig. 8.—Ansell’s Standard Gauge.]
The gauging mill is of different construction from the other mills, as
may be seen by reference to Fig. 7, where the rollers A are seen in the
act of reducing a fillet. The upper roller is fixed in brasses loosely
clamped together; the upper brass, B, being firmly bolted to the main
frame of the mill by the screws _c_, while the lower one C, which
carries the weight of the roller when it is running empty, is supported
by spiral springs shown at D. The lower roller works on a brass, E,
which rests on a wedge shown at F; the brass being cut to fit the
wedge, so that it may become similar to a solid mass, irrespective of
any motion given to the wedge. By this mode of adjusting, a difference
of the 0·001 of an inch may be made with ease between the distance
of the rollers, and, consequently, in the thickness of fillets which
may pass between them. The wedge F is moved forward and backward by
the screw G, which itself has motion from the gear work H, by the
handle I. Directly a fillet is passed between the rollers, the topmost
one is forced against its upper brasses, and further upward motion
becomes impossible. The weight of metal in this roller gives rise to
irregularities in the thickness of the fillets which pass from this
mill, causing much trouble and some expense; therefore it is proposed
to support the upper roller by a similar arrangement to that which
affects the lower roller, and to keep it rigidly against the upper
brass, but with just so much pressure as its own weight would induce
were circumstances reversed, and by these means to relieve the fillet
from the weight of the roller, because that has an undue influence on
each end of it. The gauger of fillets requires other tests besides that
of the thickness of the edge of the fillet, so he punches out a blank
from an occasional fillet by a hand-press, the cutter of which is shown
at J, Fig. 7, worked by the handle K, through the screw L. The blank
falling through the bolster of the cutter is caught at M, and is then
weighed in the hand scales N, against a standard weight, from which it
must not vary more than 0·50 grain. O, Fig. 7, is the gauge actually
used by the workman; Fig. 6 represents the standard gauge used only
by the officer in charge to check the work at its various stages. He
has in addition a gauge of great accuracy, by which to measure the
fillets at any point, as to width and thickness. This gauge will be
more intelligible by reference to Fig. 8. A is the handle, which is
hollow; B is a lever attached to the flat rod of copper C, which at D
is cut with a rack, into which a pinion E is made to work. The pinion
E works on a shaft, the upper end of which carries a hand F, provided
with a vernier G. If now the handle A be firmly held by the hand,
while the thumb be made to press the lever B towards the end of the
handle, the rod C is set in motion, and causes the hand G to travel in
the direction of H. The rod C rests on another rod I, made of steel,
and so long as to pass into the handle of the instrument. The ends of
the rods C and I are fitted at _b_ with steel shoulders, and are then
continued, as represented, to _a_. If it be desired to measure the
thickness of a fillet, the points _a a_ and _b b_ are caused to open by
pressure applied to B, and the fillet is placed between the points _a_,
when a spring fixed in the box K brings back the rod C as soon as B is
gently released, and encloses the fillet. The separation of the points
_a_ by the fillet causes the hand or indicator G to stand at a point
from zero, which is then read. The scale is divided into 500 parts;
and if the points be opened 0·50 inch, the hand makes one revolution;
so that the ·001 of an inch is gained by one reading. But each 0·001
is subdivided by the vernier into ten, so that a ten-thousandth part
of an inch is read without trouble. To measure the diameter of a blank
coin, or the width of a fillet, it must be placed between the points
_b_; but since the extreme graduation of this gauge is 0·50 inch,
it is necessary, if it be desired to measure a larger diameter, to
press back the lever B till the zero of the vernier G reaches 0·500
on the scale H, and hold it there while a clamp is made fast at the
spot indicated by the star (*), to prevent the motion of C without I.
When the clamp is fixed the rod I must be drawn out till the zero of
the vernier reaches that of the scale H, when the screws J must be
tightened to retain I in its new position, with half an inch permanent
opening between the points _b_ and between the points _a_. In a new
measurement, that permanent 0·500 must be added to the reading. This
arrangement admits of measuring up to 3·5000 inches, to which limit the
gauge is extremely accurate. The instrument was invented by myself,
because I found it difficult to convince the men that the fillet was
thickest in its middle, and consequently heavier there than it should
be; and, unfortunately, that the workmen habituated themselves to
attributing this fault to each other, when its existence was proved.
The fact was, that under the system which had prevailed, the men—with
a view to make bad work for a specially-designed reason—would set the
upper rollers at varying angles, so that a fillet at one mill would
have one thin and one thick edge; and when that fillet passed through
the next mill, the angle of the roller being altered, would make both
edges alike, but the effect of the manœuvre was to push the metal into
the middle of the fillet, and thus to unfit it for the draw-bench.
Hence the necessity to fix where the blame should rest, and the
production of this instrument, under my direction, by Mr. C. Becker, of
30, Strand, at once overcame all those difficulties.
[Illustration: Fig. 9.—Small Shears.]
[Illustration: Fig. 10.—Flatting Mill.]
The fillets are weighed from the rolling room to the drag room, where
they are finally adjusted; for with every energy, discretion, and
skill, FILLETS CANNOT BE OBTAINED OF UNIFORM THICKNESS BY SIMPLE
ROLLING. In the drag room the fillets are taken to the small shears,
Fig. 9, by which one end of each fillet is trimmed so as to render it
square. The plates A are fixed to the head of a T-shaped lever, which
is caused to oscillate by a cam beneath the floor. The plates A shut
against a face of steel fixed to a block, and held by the screws shown
at B; if therefore the end of the fillet be passed between the plate A
and the face of B, each oscillation causes the cutting off of so much
as protrudes, the pieces cut off falling into the box C, which has now
been enlarged so far as to form a pan all round the top with a view
to catch all of them. D forms part of a chain, by which the shears
are thrown out of motion. The fillets, having been trimmed so as to
render their ends square, are next passed to the extent of about two
inches between the rollers of a flatting mill, shown in Fig. 10, which
reduce that part of the fillet to about two-thirds its thickness. A
A represent a pair of small rollers, the upper one of which is cut
with three flat faces, so that it has three rounding and three flat
surfaces; hence, when both rollers are revolving, there are spaces with
openings between them; but when the rounding faces come down, those
openings are much narrowed, so that any fillet placed between them
becomes thinned to just such an extent as may be deemed necessary. The
rollers travel in opposite directions, so as to cause the expulsion
of a fillet placed between them. The reverse motion is gained as
follows:—The upper roller is driven by B, which receives its motion
from the little pinion C, carried on the shaft which also supports D.
D reverses the motion of E, which is driven from the drum F. E also
drives G, which gives motion to the lower roller. The fly-wheel H
is borne at the extreme end of the shaft which carries F and E. The
fillets are rested on J while being _flatted_, and are, after flatting,
placed in the trough K, from which they are taken to a rolling mill in
the drag room, of precisely the same construction as that exhibited at
Fig. 7, to be passed twice through at equal pinches, with a view to
render them still more accurate than they were when leaving the rolling
room, as well as to reduce them to the exact thickness at which the
trier has found they will produce the best work at the draw-bench. The
rolling mill in the drag room was provided with steel rollers. Steel
rollers are of somewhat recent invention, and seem to have received
a high character from those whose opinion may be modified by further
experiments more accurately made. My opinion, founded on experience,
is to the effect that they are not worth their extra cost; but that
their usefulness may be more fully developed when they shall have been
fitted with the arrangements proposed for the gauging mills before
explained.[19] After these alterations have been made, it may fairly
be questioned whether steel rollers will, under circumstances every
way similar, produce better work than is produced by the ordinary
chilled-iron rollers; in other words, I believe that steel is not a
better substance for rollers than chilled cast-iron. Those who have to
sell, and those who have to use, have, of course, different motives;
he who has to use a machine should judge calmly, and not be led away
because the invention is new. It is amongst these considerations that
I am convinced that steel rollers do not save money; for if they wear
longer without getting out of order, they also require a longer time
to put them again in order. Rollers, made from whatsoever substance,
cannot reasonably be expected to produce a fillet from every part of
which blanks of equal weight can be struck, because it is not yet
possible to produce a compound of equal hardness throughout; but if the
construction of the mill be altered, steel rollers may approach nearer
to that perfection which is gained by the draw-bench, but they can
never replace it. The fillets are taken from the mill to the draw-bench.
[Footnote 19: See page 23.]
[Illustration: Fig. 11.—Draw-bench.]
[Illustration: Fig. 12.—Head of Draw-bench.]
Fig. 11 represents the _draw-bench_, the name of which is retained,
as being in fact its only appropriate one. The _flatted_ end of each
fillet is passed into the opening shown at A. The _dog_ A´ is then
run up till its teeth seize the fillet. The lever is depressed until
one of the hooks O catches a bar of the circulating chain P, which
in its onward motion drags the dog, and causes it to bite the fillet
and _draw_ it through the opening at which it has been entered. P
gets its motion from a notched cam, the axle of which is shown at Q.
There are two distinct chains to each draw-bench, and there are two
distinct draw-benches, so that one description does for both double
ones. R is a cogged wheel, the shaft of which, Q, carries two notched
drums, and each drum gives motion to a chain, so that both chains
travel at the same pace. R is set in motion by the pinion S, on the
shaft which is driven by the wheel T. T is driven by U, which is on
the shaft driven by the strap and drums V. Fig. 12 is a representation
of the head of the draw-bench, and in studying this engraving it will
be well to refer at the same time to Fig. 11. The dog takes its name
from its resemblance to the head of a bull-dog. It consists of a pair
of levers, whose long arms extend beyond the axle-tree of the wheels
nearest to O, and whose shortest arms are formed by the passing of the
other axle-tree through the lever. The teeth are set at the front of
the short arms. The axle-tree near O is fixed to the bars forming O,
and runs loosely between the long arms of the lever, so that when O is
pulled forcibly it causes the axle-tree to open the long end of the
levers, and thereby to close the short end or teeth of the dog, the
more rigidly in proportion to the pressure exerted at O. Directly the
fillet has passed through the cylinders the dog springs slightly by the
elasticity of the fillet, and thus releases itself from the chain; at
the instant of release the weight over the foremost wheels falls, and
by its fall lifts the hooks O so high as to admit of their escaping
contact with the circulating chain P. The position of the teeth of
the dog is shown by A in Fig. 12. The flatted part of the fillet is
just so thin as to admit of its passing easily between the cylinders
B until seized by A, but the part which is not thinned comes against
the cylinders B, and requires considerable force to drag it between
them. The cylinders B do not rotate; in fact, they may be considered as
forming part of a solid mass.[20] The lower cylinder is laid on the bed
C, and is clamped there by a cheek fastened on to C by three screws,
the holes for which are shown on C; the upper cylinder is fixed to
the mass D by a precisely similar arrangement. The beds C D are held
perpendicularly by the points of the screws E; and we may now view the
cylinders as secured to, and forming part of, their beds. The distance
between the cylinders is regulated by the capstans F, which separate
the beds of the cylinders, and so separate the cylinders. The accuracy
of this adjustment is all-important, because the distance between the
cylinders determines the thickness of the fillet which passes between
them. The bed D of the upper cylinder is required to be movable at
pleasure; it is therefore provided at G with four wedges, two of which,
_c c_, are cut so that if looked upon from the top a round hole shows
itself, and through this hole the end of the screw, which at this
point L is plain, and has a neck turned in it, passes, with its head
beneath the wedges and against the lower G. So soon as this is effected
the wedges A B are pressed into their places, and these holding _c c_
together, cause them to secure G by its neck; if, therefore, G be now
caused to rise, the block D must rise with it, but the head of this
screw rests on the solid block D, while its neck is just so long as
to admit of this without itself being pressed against the wedges _c
c_. G is a very fine-cut screw which fits into a female screw cut in
the frame of the head of the draw-bench; it is moved to any distance
varying from the hundred-thousandth part of an inch (0·00001) and
upwards by the wheel H, which receives a very minute motion from the
pinion I by means of a lever fitting into the capstan head J. K was
originally intended to be used to set or fix the screw G when it had
been brought to its proper position, but it is not used; for, in fact,
the cylinders wear away appreciably by the passage of the fillets, so
that they constantly require to be brought nearer together to make up
for this wear. With some species of gold the friction is so great that,
although oil is used, the cylinders become so hot as to render the
gold pasty; in such case a kind of welding takes place, which causes
the tearing of the fillet. If this extreme point be not reached, as
indeed it seldom is, the cylinders become of varying temperatures,
and so great is the effect of this, that in order to compensate for
it, the upper cylinder has to be continually raised or depressed. The
beds which carry the cylinders become worn by the strain and fret,
and require grinding out at intervals; therefore, to allow for the
difference which this would make, screws N are provided, by which the
cylinder in the lower bed can always be raised to its proper position.
We cannot but admire the ingenious productions of inventive minds;
and surely if ever there were a marvellous machine for assisting the
coiner, it is this; indeed, it may be doubted whether a more admirable
instrument for its purpose can be contrived. Sir John Barton, who
invented and directed the making of it, took into consideration every
circumstance which could possibly arise, but he never saw practically
the full advantage of his conception. Under my direction, this machine
was so used that the average work produced was very favourably compared
with the trials recorded by Sir John Barton, and details of which were
given to me by the late Mr. W. H. Barton. There are some persons who
smile at the draw-bench, but it is one of those inventions which will
outlive its detractors, at least, so long as economy and perfection
are points to be studied in coining. Foreign Mints are said to have
found no advantage in the use of the draw-bench. It is to be regretted
that they have not found a man with sufficient intelligence to use
so accurate an instrument; it is surely not the fault of the sun if
men are blind to its splendour. Mr. J. Martin, of the Paris Mint, has
recently made some very accurate experiments with the draw-bench,
and has produced results every way in accordance with those obtained
by me in the Royal Mint, and is convinced that the draw-bench may be
considered as the coiner’s right hand.
[Footnote 20: As the cylinder wears, the screws of C may be loosened
to permit the shifting of the abraded part, so that the whole
circumference of the cylinder may be used.—See also page 31.]
Against all sound advice the Master had been induced to buy a pair of
steel rollers, at a cost of £800 (I state the sum on the authority of
Mr. W. H. Barton, who, being Comptroller at the time, probably knew the
actual cost), and with these I made an elaborate series of experiments,
extending over many weeks. The results were wholly adverse to the
new rollers—others arrived at the same conclusion—and I reported to
the Master, in writing, on the facts as I found them, showing that
the average gave an advantage of 19·92 per cent. in favour of the
draw-bench, and on this ground I maintained the superiority of that
machine. He replied by a peremptory order, directing me “to prohibit
now and for ever” the “use of the draw-bench, and to take measures for
its removal from the Mint.” Thus absolved from responsibility, I—after
making a written protest—obeyed that which I could no longer withstand.
The result was that the rejected blanks, which had averaged 3·60 per
cent., now advanced to 23·52 per cent. I was unable to avoid this great
expense, and when I spoke to him about it he was not very amiably
disposed; however, he finally wrote me the following note, on which I
remarked to him “that steel rollers, whether driven by cogged wheels or
by straps, would still be steel rollers.”
“_7th June, 1861._
“DEAR SIR,
“In the cutting and adjusting room you may return to the use of
the draw-bench till the gearing of the steel rollers is altered.
I had overlooked the circumstance that in the United States Mint
cogged wheels are not used for that purpose.
“Yours truly,
“THO. GRAHAM.
“G. F. Ansell, Esquire.”
It is satisfactory to me to find that Mr. Fremantle confirms the
opinion at which I had arrived. He says (“European Mints,” page
9):—“The adjustment of the fillets after rolling is in some European
Mints performed by the draw-bench, as in England. In others it is
performed by carefully adjusted rolling mills only. The experience
acquired both in this country and abroad tends to show that it is
advisable to retain the draw-bench—at any rate, until some more
accurate method is found of equalising the fillets and reducing them
to their correct thickness.” If Mr. Fremantle will investigate for
himself instead of being guided by the opinions of others, he will
rigidly follow the correct conclusion at which he has arrived; if,
however, he will look in the drag room in the Royal Mint, he will
discover evidence of the former existence of a series of rollers which
were replaced by the draw-bench. Yet one of his co-travellers, who is
manifestly willing to make experiments, says of the draw-bench, “Still
it has yet to be proved that it can compete in sustained accuracy
with a well-constructed rolling mill.” Quite true; but I think the
answer holds good, and any one who would replace the draw-bench by
rolling mills—which have hitherto failed—should, as Sir John Barton
did, prove his proposition otherwise than at the Government expense,
and then on success obtain fair remuneration. Before leaving the study
of this instrument it is right that I should mention that Mr. John
Murray, of the Royal Mint, has added immeasurably to the value of
it by inventing a most ingenious machine for grinding the cylinders
(see B, page 28) with accuracy, so that those cylinders which have
been used can with ease be, as it were, repaired. In justice to Mr.
Murray I should add that I omitted all mention of his invention in any
former issue, because some principal contractors were to my knowledge
intending to make him an offer of a sum of money for it, and under such
circumstances I could not think it right to give a description of it. A
like feeling induces me to postpone to another occasion details of this
clever contrivance; its simplicity is such that a mere outline would
put a maker of instruments in possession of means for its construction.
The fillets which have passed between the draw-bench cylinders are cut
into lengths of about 18 inches by the shears shown at X, in Fig. 11,
and are then sent to the trier, who by means of a hand-press similar
to, but more delicate than, that shown at Fig. 7, punches out one or
two blanks from each length of 18 inches, and weighs it, or them,
against a standard weight, and in accordance with his judgment directs
the fillets to be cut by the boys or men at the machines. The trier
allows 0·20 grain on the pound of blanks for the loss which afterwards
occurs by annealing.[21] If, however, the bars, as previously
suggested, were cast uniformly of the thickness of 0·50 inch, this
allowance, which is equal to a value of £34 8_s._ 7½_d._ on each
million, need not be made; but in fact, as will be seen, even this is
not sufficient to cover that loss under present circumstances.
[Footnote 21: See page 48.]
Not only has it become a habit to smile at the draw-bench, but every
unfair attempt has been made to get rid of it. Officers were abused
because they would not report against it, and the machine itself was
submitted to usage never contemplated by the inventor. The then chief
coiner, who had formerly seen soap used in calico works in Manchester,
insisted on using soap-suds, whereby the beds for the cylinders became
rusted, the cylinders destroyed, and the whole machine thrown out
of gear, so that 30 per cent. of all the work was rejected: these
perverse trials, extending over weeks, appeared to throw discredit on
the draw-bench. Having been a calico-printer, that officer endeavoured
to engraft on to the processes of coining some of the practices
adopted in that business; but had he duly appreciated the principle
on which the draw-bench acts, he could not have attempted the use of
soap-suds, or, at least, on its complete failure would have assented
to its disuse. The very first object of the draw-bench is to produce
just so much friction as will cause the lateral displacement of the
molecules of the metal then under its operation. Soap, when it adheres
to the bullion, permits the fillet to pass without friction, and
when it is scraped off by the cylinders the gold becomes so hot from
friction that the hand cannot with safety touch it; hence there are
alternating parts of the fillet very hot and absolutely cold, and, as
a consequence, no two blanks can be obtained of equal weight. Sir John
Barton not only made the machine, but determined also that oil was
the only fit lubricator for metal made to pass through the cylinders
of the draw-bench. Forgetful of the immediate wear on the surface of
the metal, others have attempted to replace the cylinders by wedges of
steel, so made as that a constant stream of cold water should keep them
cool when in operation. This also failed from the formation of rust,
while the work produced never equalled that obtained from cylinders.
The proper use of the draw-bench is to reduce fillets to an equable
thickness in every part, and this can only be done when the trier,
after studying the quality of his metal, has determined how much he
can remove by once passing through the cylinders; then by keeping up
a constant succession of fillets, properly smeared with oil, so that
the equable friction always maintains them at the same temperature.
Under such circumstances, and with a remedy of 0·24 grain, the rejected
should not exceed 2 per cent., and this on the whole day’s work should
contain half its weight of light and the other half heavy blanks. This
also was a curious instance of want of knowledge on the part of that
controlling officer, who for years maintained that if the work were
properly conducted _all the rejected_ should be on one side of the
remedy.[22] The fillets, notwithstanding the draw-bench, cannot be
brought to perfect accuracy, and to meet such variations as arise, a
difference is made in two of the cutting-out punches by altering their
diameters to such an extent that a blank cut by them from a standard
fillet would vary in weight from a blank cut by a standard cutter from
the same fillet. One cutting-out punch is so altered that a blank
would be 0·125 grain, and the other that a blank would be 0·250 grain
heavier. This admits of a fillet otherwise too thin being used; but if
the fillet be found to err on the other side, it is passed once more
either through the draw-bench, or through the mill at a spring-pinch.
The trier, Mr. William Fenton, is a peculiarly steady man, possessing
a calm judgment, with considerable energy, and upon him depends the
accuracy of the whole process of coining; he has not unfrequently so
managed his work that upon 5,000,000 of sovereigns coined, he has been
within one sovereign of the calculated value.
[Footnote 22: See page 39.]
The fillets, having been thrown by the trier into the receptacles which
indicate the particular cutting-out punches to which they are to be
taken, are fetched by a man, who wipes off the oil, and then carries
them to the cutting-out room, where the fillets are cut into blanks
and scissel. In this place it may farther be noticed that soap-suds
cannot be used in the place of oil, because the soap could not be
removed without washing,—a practical impossibility,—and would therefore
remain, and add indefinitely to the weight of the gold, and thus open
the door for peculation. The cutting-out presses used in the Royal Mint
are very cumbersome, and when in operation are terribly noisy: it is
therefore hoped that at no distant period they may be replaced by some
of a far more simple construction; but it is believed that under all
circumstances it will be found wise to adhere to the plan of cutting
out a single blank at each descent of the punch.[23] For bronze it
is well to obtain five or more blanks at each blow, but the limited
variation of weight allowed by law on blanks of the precious metals
would render this false economy. Fig. 13 represents one of the twelve
cutting-out presses, which are all driven by the wheel A, provided
with a series of cams on its outer rim; one of these cams, B, is in
the act of striking the friction roller C, which is attached to, and
forms part of, the lever D. D is fixed to an upright shaft E, which
at F is cut with a screw thread working into a female screw fitted
into the main shoulder of the press at G. If now the cam B strikes
C, and throws it outwards, it causes the shaft E to take a part of a
revolution, and in so doing the screw F makes it rise and carry with
it the block H, whose tendency to circular motion is prevented by a
plug fitting into its groove, and fixed in the guide I. The lower end
of H carries the screwed cap J, which supports the cutting-out punch,
so that when E rises it carries the cutting-out punch through just the
same distance that itself travels upwards. The cutting-out punch is
now ready for action, and is released by the continued revolution of
the wheel A, as will be seen by the figure; but as it could not fall
with sufficient force of itself, assistance is rendered by the pressure
of the atmosphere, as will be seen by the following arrangement. The
lever D is provided, near its junction at E, with a loop of iron
travelling on a screw, so that it may be moved farther from, or nearer
to, the centre of action, and thus admit of the increase of power.
This loop of iron is represented by K, and is continued by a rod of
iron across the upper part of the room and through a hole in the wall
to a system of levers L, from which a rod is suspended, the lower end
being connected with a piston working in the chamber M. The chamber M
is an hermetically-closed vessel secured to a stone firmly fixed in the
floor. The piston works in this chamber, and is covered with about two
inches of oil, which prevents the access of the atmosphere by leaks to
any part beneath the piston. If the piston, therefore, be raised from
the base of the chamber, a vacuum is produced in that portion from
which the piston is removed, and consequently the atmosphere presses
on the surface of the oil, which in its turn presses on the piston,
and carries it down (the reverse of the action explained by Mr. James
Napier in “European Mints”); in its fall the piston pulls down the
cutter, which has been raised; for the same blow which raises the
cutter also raises this piston; therefore, when the cutter is raised
the workman places the fillet N, from which blanks are to be cut, on
the bolster, shown at O, and holds it firmly while the cutter descends
and punches out a blank, which falls through the bolster into the
drawer P. By the time that the down stroke of the cutting-out punch is
complete, the wedge Q has entered a slit in the spring R, and strikes
the spring, thus throwing the
Cite this